FabDigit

Copper Alloy CC494K

EN CC494K

CC494K (CuSn5Pb9-C, C93400) is a high-lead, low-tin cast bronze whose 8–11 % free lead provides self-lubrication and a machinability rating of 90.

High cost $$$$

Reference datasheet — CC494K is not in the instant-quote catalog. Upload your part and an engineer will quote it in this grade or suggest the closest stocked equivalent.

Values for the GC condition

CC494K tempers and conditions

CC494K is supplied in 4 conditions, soft to hard. GC is the default FabDigit quotes; the values on this page are for it.

Compare all 4 conditionsHide
Condition · open for datasheetBest forYield MPaTensile MPaElong. %HardnessConductivity
Sand cast
Choose for one-off or large, complex bearing housings and pump parts where section size rules out chill or continuous casting.851801062 HB15 % IACS
Chill / permanent-mould cast
Choose for medium-volume small bushings needing finer grain, tighter tolerance and slightly higher strength than sand casting.95200865 HB15 % IACS
Centrifugally cast
Choose for large-diameter, thick-wall bushings and slide rings where a dense, porosity-free wall is required.1002151065 HB15 % IACS
GCDefault
Continuously cast bar / tube
Default stock form: continuous-cast round bar and hollow bar for machined bushings, thrust washers and wear strips.1052201068 HB15 % IACS

What is CC494K?

CC494K (CuSn5Pb9-C, C93400) is a high-lead, low-tin cast bronze whose 8–11 % free lead provides self-lubrication and a machinability rating of 90. It is specified for moderately loaded bearings and bushings at 105 MPa yield, 220 MPa tensile, 10 % elongation and 68 HB, supplied as sand (GS), chill (GM), centrifugal (GZ) and continuous (GC) castings, with continuous-cast tube commonly bored to size. The low tin content limits load and fatigue capacity, and the lead makes the alloy unweldable and unsuitable for lead-restricted plumbing; CC493K (C93200) is the stronger alternative. CC494K has a density of 8.9 g/cm³ (0.322 lb/in³), heavier than 77% of copper alloy grades. It melts at 855°C (1,571 °F). CC494K has a yield strength of 105 MPa (15.2 ksi) and a tensile strength of 220 MPa (31.9 ksi) — weaker than 85% of copper alloy grades. Elongation at break is 10% and the elastic modulus is 80 GPa (11.6 Msi).

What is CC494K used for?

  • bushings
  • bearings
  • low-speed sliding components
  • hydraulic fittings

Advantages

  • Easy to machine — 90/100, better than 98% of copper alloy grades

Limitations

  • Hard to polish — 50/100, worse than 99% of copper alloy grades
  • Low stiffness — 80 GPa (11.6 Msi), worse than 97% of copper alloy grades
  • Difficult to weld — 12/100, worse than 96% of copper alloy grades
  • Limited formability — 8/100, worse than 94% of copper alloy grades
  • Low strength — 105 MPa (15.2 ksi), worse than 85% of copper alloy grades

CC494K properties

Typical room-temperature values for CC494K-GC; bars are the position among copper alloy grades.

Physical3

CC494K has a density of 8.9 g/cm³ (0.322 lb/in³), heavier than 77% of copper alloy grades. It melts at 855°C (1,571 °F).

Density8.9 g/cm³0.32 lb/in³
Melting Point (Solidus)855°C1,571 °F
Liquidus Temperature1,000°C1,832 °F

Mechanical15

CC494K has a yield strength of 105 MPa (15.2 ksi) and a tensile strength of 220 MPa (31.9 ksi) — weaker than 85% of copper alloy grades. Elongation at break is 10% and the elastic modulus is 80 GPa (11.6 Msi).

Elastic (Young's) Modulus80 GPa11.6 Msi
Shear Modulus30 GPa4.4 Msi
Bulk Modulus105 GPa15.2 Msi
Poisson's Ratio0.34
Tensile Strength (Ultimate)220 MPa31.9 ksi
Yield Strength (0.2% offset)105 MPa15.2 ksi
Elongation at Break10%
Reduction in Area14%
Compressive Strength230 MPa33.4 ksi
Shear Strength150 MPa21.8 ksi
Fatigue Strength (Endurance Limit)72 MPa10.4 ksi
Charpy V-Notch Impact (RT)11 J8.1 ft·lbf
Hardness, Brinell68 HB
Hardness, Rockwell B24 HRB
Hardness, Vickers72 HV

Thermal6

CC494K is rated for continuous service to 200°C (392 °F). It conducts heat at 71 W/m·K (41 BTU/hr·ft·°F), worse than 54% of copper alloy grades. Thermal expansion is 18 µm/m·K (10 µin/in·°F).

Thermal Conductivity71 W/m·K41 BTU/hr·ft·°F
Specific Heat Capacity377 J/kg·K0.09 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)18 µm/m·K10 µin/in·°F
Latent Heat of Fusion170 J/g73.1 BTU/lb
Max Service Temperature (continuous)200°C392 °F
Min Service Temperature-100°C-148 °F

Electrical3

CC494K conducts electricity at 15 % IACS, worse than 54% of copper alloy grades.

Electrical Conductivity15 % IACS
Electrical Resistivity1.15×10⁻⁷ Ω·m4.53 µΩ·in
Magnetic Responsenon-magnetic

Chemical & Environmental3

Corrosion resistance is good (60/100), worse than 68% of copper alloy grades.

Galvanic Potential (seawater, vs SCE)-0.26 V
Corrosion ResistanceGood60/100
Chemical Resistance SummaryGood in fresh and low-velocity sea water, neutral salts, mineral oils, steam and industrial atmospheres; attacked by ammonia/amines (SCC risk), oxidising and strong mineral acids, and lead can leach in acidic potable water.

Sustainability4

Producing a kilogram of CC494K takes about 60 MJ of energy and emits 4 kg of CO₂ — more than 69% of copper alloy grades. Typical recycled content is 60%.

Embodied Energy (primary production)60 MJ/kg25,795 BTU/lb
Embodied Carbon (primary production)4 kg CO₂/kg
Embodied Water250 L/kg30 gal/lb
Typical Recycled Content60%

Manufacturability8

CC494K's machinability is excellent (90/100, better than 98% of copper alloy grades); weldability not recommended (12/100); formability not recommended (8/100).

MachinabilityExcellent90/100
Machinability Rating (AISI 1212 = 100 %)82%
WeldabilityNot recommended12/100
Formability (cold)Not recommended8/100
CastabilityVery good82/100
Brazeability / SolderabilityFair40/100
PolishabilityFair50/100
Anodizing Responsen/a — copper alloy; use chemical patination, tin or nickel plating instead

Common Calculations5

Specific Strength (UTS / density)calculated25 kN·m/kg
Specific Stiffness (E / density)calculated9 MN·m/kg
Modulus of Resiliencecalculated69 kJ/m³
Thermal Diffusivitycalculated21.2 mm²/s
Thermal Shock Resistance Indexcalculated11

Values are nominal handbook figures for design screening. Certified mill or lot data ships with every FabDigit order on request.

Strength versus weight in the copper alloy family

Yield strength against density for every copper alloy grade FabDigit runs. CC494K is highlighted; hover a dot for its name, or open the interactive family chart.

501002005001,0007.588.599.5Density (g/cm³)Yield strength (MPa) — log scaleCC494K

Working with CC494K

Is CC494K easy to machine?

Excellent free-cutting behaviour with short chips — use sharp positive-rake carbide or HSS, 0° to slightly negative rake for interrupted cuts, high speed and light feed; capture lead-bearing swarf for controlled disposal.

Can CC494K be welded?

Essentially unweldable by fusion processes due to 8–11% Pb (hot cracking, lead fume); repair by soft soldering or mechanical means, or use low-Pb bronze if welding is required.

Can CC494K be formed, bent or molded?

Cast-only alloy with a wide freezing range — feed generously with chills and risers to avoid inverse segregation and lead sweat; not cold formable, light coining/broaching of bores only.

CC494K chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
Sn4 – 65
Pb8 – 119
Zn≤ 21
Niincluding Co≤ 2
Sb≤ 0.5
Fe≤ 0.3
P≤ 0.1
S≤ 0.1
Mn≤ 0.2
Al≤ 0.01
Si≤ 0.01
Cu≥ 83 (balance)

What surface finishes work on CC494K?

Bore-size finishing by fine boring, reaming, roller burnishing or honing; tin or nickel plating for potable-water and appearance work, chemical patination for decorative parts, high mirror polish limited by lead smear.

Surface treatments FabDigit runs on copper alloy parts — pick them in the quote configurator or call them out on the drawing. Each links to its datasheet in the surface-finish library (thickness, specs, call-out, material verdicts).

Equivalent designations

Standards and trade names that resolve to Copper Alloy CC494K in FabDigit's catalog. Equivalence is nominal — check the exact specification when certification matters.

EN / DIN / Werkstoff-Nr.
CuSn5Pb9-C
Similar grades
C93400

How much does CC494K cost?

CC494K is a high-cost copper alloy ($$$$), pricier than about 78% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

CC494K — frequently asked

What is CC494K used for?

CC494K is typically used for bushings, bearings, low-speed sliding components and hydraulic fittings. In short: highest machinability cast bronze; low-load bearing alloy; strong self-lubricating action.

What is the yield strength of CC494K?

CC494K has a typical yield strength of 105 MPa (15.2 ksi) and a tensile strength of 220 MPa (31.9 ksi) — weaker than 85% of copper alloy grades. Strength varies by condition: see the 4 listed tempers.

Is CC494K easy to machine?

Yes — machinability is rated excellent (90/100, better than 98% of copper alloy grades). Excellent free-cutting behaviour with short chips — use sharp positive-rake carbide or HSS, 0° to slightly negative rake for interrupted cuts, high speed and light feed; capture lead-bearing swarf for controlled disposal.

Can CC494K be welded?

Not readily — weldability is rated not recommended (12/100). Essentially unweldable by fusion processes due to 8–11% Pb (hot cracking, lead fume); repair by soft soldering or mechanical means, or use low-Pb bronze if welding is required.

What surface finishes work on CC494K?

Bore-size finishing by fine boring, reaming, roller burnishing or honing; tin or nickel plating for potable-water and appearance work, chemical patination for decorative parts, high mirror polish limited by lead smear.

Can CC494K be formed, bent or molded?

Cast-only alloy with a wide freezing range — feed generously with chills and risers to avoid inverse segregation and lead sweat; not cold formable, light coining/broaching of bores only.

What is the maximum service temperature of CC494K?

CC494K is rated for continuous use to about 200°C (392 °F). Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

What is the difference between CC494K-GC and CC494K-GS?

GC is the default condition — default stock form: continuous-cast round bar and hollow bar for machined bushings, thrust washers and wear strips. GS: choose for one-off or large, complex bearing housings and pump parts where section size rules out chill or continuous casting. Yield strength is 105 MPa in GC versus 85 MPa in GS.

How much does CC494K cost?

CC494K is a high-cost copper alloy ($$$$), pricier than about 78% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

Sources

  1. EN 1982 — Copper and copper alloys: Ingots and castings (CuSn5Pb9-C / CC494K) — CEN (2017)
  2. ASTM B505/B505M — Continuous Cast Copper Alloys — ASTM International (2022)
  3. CDA Alloy Database — C93400 / C93500 leaded tin bronze — Copper Development Association (2023)
  4. ASM Handbook Vol. 2 — Properties and Selection: Nonferrous Alloys — ASM International (1990)
  5. DKI Informationsdruck — Guss aus Kupferlegierungen — Deutsches Kupferinstitut (2012)

Property data is compiled from published supplier and standards handbooks and normalised for comparison; hardness values on non-Brinell scales are converted approximately for charting only. Manufacturability limits are FabDigit quote-engine defaults and may be relaxed by engineering review. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.