Titanium Ti Grade 31 CW-SR

Supply condition

UNS R53532 · ASTM Grade 31

CW-SR = cold Worked + Stress Relieved

Choose for higher strength and tighter tolerance fasteners, shafts and instrument tubing.

High cost $$$$

Values for the CW-SR condition

Other Ti Grade 31 tempers and conditions

Ti Grade 31 is listed in 2 conditions; see the grade overview at Ti Grade 31.

Compare all 2 conditionsHide
Condition · open for datasheetBest forYield MPaTensile MPaElong. %HardnessConductivity
AnnealedDefault
mill annealed sheet, plate, bar, tube
Default stocked condition for heat-exchanger tube, plate and vessel linings in hot brines.45055022200 HB—
CW-SRThis page
Cold Worked + Stress Relieved
Choose for higher strength and tighter tolerance fasteners, shafts and instrument tubing.6006901322 HRC3 % IACS

What is Ti Grade 31 CW-SR?

Ti Grade 31 CW-SR is Ti Grade 31 supplied in the CW-SR condition — choose for higher strength and tighter tolerance fasteners, shafts and instrument tubing. Ti Grade 31 CW-SR has a yield strength of 600 MPa (87 ksi) and a tensile strength of 690 MPa (100 ksi) — stronger than 50% of titanium grades. Elongation at break is 13% and the elastic modulus is 105 GPa (15.2 Msi). Ti Grade 31 CW-SR has a density of 4.51 g/cm³ (0.163 lb/in³), heavier than 57% of titanium grades. It melts at 1,650°C (3,002 °F). Annealed is the default condition FabDigit quotes; CW-SR is available on request or by drawing note.

Advantages

  • Conducts heat well — 17 W/m·K (9.82 BTU/hr·ft·°F), better than 84% of titanium grades
  • Easy to machine — 35/100, better than 78% of titanium grades

Limitations

  • Limited service temperature — 250°C (482 °F), worse than 99% of titanium grades
  • Low fracture toughness — 55 MPa·√m (50.1 ksi·√in), worse than 90% of titanium grades

Ti Grade 31 CW-SR properties

Typical room-temperature values for Ti Grade 31 CW-SR; 23 are specific to this condition. Other listed values are Ti Grade 31 reference data and may not represent this condition. Bars are the position among titanium grades.

Physical3

Ti Grade 31 CW-SR has a density of 4.51 g/cm³ (0.163 lb/in³), heavier than 57% of titanium grades. It melts at 1,650°C (3,002 °F).

Density4.51 g/cm³0.16 lb/in³
Melting Point (Solidus)1,650°C3,002 °F
Liquidus Temperature1,670°C3,038 °F

Mechanical16

Ti Grade 31 CW-SR has a yield strength of 600 MPa (87 ksi) and a tensile strength of 690 MPa (100 ksi) — stronger than 50% of titanium grades. Elongation at break is 13% and the elastic modulus is 105 GPa (15.2 Msi).

Elastic (Young's) Modulus105 GPa15.2 Msi
Shear Modulus45 GPa6.5 Msi
Bulk Modulus110 GPa16 Msi
Poisson's Ratio0.34
Tensile Strength (Ultimate)690 MPa100 ksi
Yield Strength (0.2% offset)600 MPa87 ksi
Elongation at Break13%
Reduction in Area30%
Compressive Strength630 MPa91.4 ksi
Shear Strength450 MPa65.3 ksi
Fatigue Strength (Endurance Limit)350 MPa50.8 ksi
Fracture Toughness (K_IC)55 MPa·√m50.1 ksi·√in
Charpy V-Notch Impact (RT)16 J11.8 ft·lbf
Hardness, Brinell240 HB
Hardness, Rockwell B100 HRB
Hardness, Vickers252 HV

Thermal6

Ti Grade 31 CW-SR is rated for continuous service to 250°C (482 °F). It conducts heat at 17 W/m·K (9.82 BTU/hr·ft·°F), better than 84% of titanium grades. Thermal expansion is 8.6 µm/m·K (4.78 µin/in·°F).

Thermal Conductivity17 W/m·K9.8 BTU/hr·ft·°F
Specific Heat Capacity523 J/kg·K0.12 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)8.6 µm/m·K4.8 µin/in·°F
Latent Heat of Fusion365 J/g157 BTU/lb
Max Service Temperature (continuous)250°C482 °F
Min Service Temperature-250°C-418 °F

Electrical3

Ti Grade 31 CW-SR conducts electricity at 3 % IACS, better than 60% of titanium grades.

Electrical Conductivity3 % IACS
Electrical Resistivity5.8×10⁻⁷ Ω·m22.8 µΩ·in
Magnetic Responsenon-magnetic

Chemical & Environmental3

Corrosion resistance is excellent (95/100), better than 83% of titanium grades.

Galvanic Potential (seawater, vs SCE)-0.1 V
Corrosion ResistanceExcellent95/100
Chemical Resistance SummaryOutstanding in seawater, wet chlorine, hypochlorite, oxidizing acids and hot chloride brines; the Pd+Co addition suppresses crevice corrosion in low-pH, high-temperature brines up to ~250–300 °C where Grade 2/3 fail. Attacked by HF, dry chlorine, red fuming nitric acid, anhydrous methanol and hot concentrated reducing acids.

Sustainability4

Producing a kilogram of Ti Grade 31 CW-SR takes about 650 MJ of energy and emits 40 kg of CO₂ — less than 75% of titanium grades. Typical recycled content is 30%.

Embodied Energy (primary production)650 MJ/kg279,450 BTU/lb
Embodied Carbon (primary production)40 kg CO₂/kg
Embodied Water1,500 L/kg180 gal/lb
Typical Recycled Content30%

Manufacturability8

Ti Grade 31 CW-SR's machinability is fair (35/100, better than 78% of titanium grades); weldability very good (80/100); formability poor (30/100).

MachinabilityFair35/100
Machinability Rating (AISI 1212 = 100 %)28%
WeldabilityVery good80/100
Formability (cold)Poor30/100
CastabilityPoor30/100
Brazeability / SolderabilityFair40/100
PolishabilityVery good70/100
Anodizing Responsegood — colour (interference) anodizing per AMS 2488 type II gives decorative/anti-gall oxide; not a corrosion-critical layer since the base metal is already passive

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with Ti Grade 31 CW-SR

Is Ti Grade 31 easy to machine?

Machine like CP Ti Grade 3: rigid setup, sharp uncoated-carbide or PVD tools, low surface speed (25–45 m/min), heavy positive rake, generous flood coolant to avoid galling and chip ignition.

Can Ti Grade 31 be welded?

Excellent GTAW/PAW/EBW weldability with matching or Grade 2/7 filler; requires full inert-gas shielding of pool, trailing shield and backing, and a clean, oxide-free joint (straw/blue tint = reject).

Can Ti Grade 31 be formed, bent or molded?

Cold form with generous bend radii (≈3–4t) and allow for high springback; warm forming at 200–400 °C markedly improves formability; never form with iron-contaminated tooling.

What surface finishes work on Ti Grade 31?

Pickle in HNO₃/HF to remove alpha case and embedded iron; can be colour-anodized per AMS 2488, glass-bead blasted, or polished — no protective coating is needed for corrosion.

Ti Grade 31 chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
Pdpalladium micro-addition for crevice-corrosion resistance0.04 – 0.080.05
Cocobalt co-addition, cathodic modifier0.2 – 0.80.35
Fe≤ 0.30.15
Ohigher-oxygen (higher strength) member of the Gr.30/31 pair≤ 0.350.25
C≤ 0.080.02
N≤ 0.050.02
Hmax (0.0125 for billet/bar in some forms)≤ 0.020.01
Residuals (each)total 0.40 max≤ 0.1—
Tibalance—

Ti Grade 31 CW-SR — frequently asked

What is Ti Grade 31 CW-SR used for?

Ti Grade 31 CW-SR is typically used for formed chemical process components, corrosion-resistant tubing and welded tube, reactor and vessel internals, seawater and brine piping fittings, heat-exchanger plates and shells and drawn and pressed tank heads. In short: low-interstitial Grade 30; formable crevice-resistant titanium; higher strength than CP grades.

What is the yield strength of Ti Grade 31 CW-SR?

Ti Grade 31 CW-SR has a typical yield strength of 600 MPa (87 ksi) and a tensile strength of 690 MPa (100 ksi) — stronger than 50% of titanium grades. Strength varies by condition: see the 2 listed tempers.

Is Ti Grade 31 CW-SR easy to machine?

Not especially — machinability is rated fair (35/100, better than 78% of titanium grades). Machine like CP Ti Grade 3: rigid setup, sharp uncoated-carbide or PVD tools, low surface speed (25–45 m/min), heavy positive rake, generous flood coolant to avoid galling and chip ignition.

Can Ti Grade 31 CW-SR be welded?

Yes — weldability is rated very good (80/100). Excellent GTAW/PAW/EBW weldability with matching or Grade 2/7 filler; requires full inert-gas shielding of pool, trailing shield and backing, and a clean, oxide-free joint (straw/blue tint = reject).

What surface finishes work on Ti Grade 31 CW-SR?

Pickle in HNO₃/HF to remove alpha case and embedded iron; can be colour-anodized per AMS 2488, glass-bead blasted, or polished — no protective coating is needed for corrosion.

Can Ti Grade 31 CW-SR be formed, bent or molded?

Cold form with generous bend radii (≈3–4t) and allow for high springback; warm forming at 200–400 °C markedly improves formability; never form with iron-contaminated tooling.

What is the maximum service temperature of Ti Grade 31 CW-SR?

Ti Grade 31 CW-SR is rated for continuous use to about 250°C (482 °F). Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

What is the difference between Ti Grade 31 Annealed and Ti Grade 31 CW-SR?

Annealed is the default condition — default stocked condition for heat-exchanger tube, plate and vessel linings in hot brines. CW-SR: choose for higher strength and tighter tolerance fasteners, shafts and instrument tubing. Yield strength is 450 MPa in Annealed versus 600 MPa in CW-SR.

Sources

  1. ASTM B265 — Titanium and Titanium Alloy Strip, Sheet, and Plate — ASTM International (2020)
  2. ASTM B348 — Titanium and Titanium Alloy Bars and Billets — ASTM International (2021)
  3. ASTM B338 / B337 — Seamless and Welded Titanium Tube and Pipe for Condensers and Heat Exchangers — ASTM International (2021)
  4. ASM Handbook Vol. 2 — Properties and Selection: Nonferrous Alloys (Titanium) — ASM International (1990)
  5. ASM Handbook Vol. 13B — Corrosion: Materials (Titanium) — ASM International (2005)
  6. Pd/Co-enhanced corrosion-resistant CP titanium product data — TIMET / Titanium Metals producer literature (2019)

Property data is compiled from published supplier and standards handbooks and normalised for comparison. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.