FabDigit

Rigur

also RGD450

Rigur (RGD450) is a polypropylene-simulating PolyJet photopolymer and the tougher, more impact-resistant successor to Durus, available in glossy, matte and digital-material blends.

High cost $$$$

Reference datasheet — Rigur is not in the instant-quote catalog. Upload your part and an engineer will quote it in this grade or suggest the closest stocked equivalent.

Values for the RGD450 condition

Rigur grades and fills

Rigur is supplied in 3 conditions, soft to hard. RGD450 is the default FabDigit quotes; the values on this page are for it.

Compare all 3 grades and fillsHide
Grade · open for datasheetBest forYield MPaTensile MPaElong. %Hardness
Rigur + rubber-like/rigid partner resin
Use on Connex multi-material machines when a softer, higher-elongation PP-like feel or graded stiffness in one part is required.22306065 Shore D
RGD450Default
Rigur white, standard PolyJet build
Default white Rigur cartridge printed on Objet/Connex PolyJet systems for PP-like functional prototypes.38423280 Shore D
Glossy print state
Choose when smooth, near-molded surface finish and slightly higher measured strength on skin surfaces are wanted.40443581 Shore D

Supply forms, finishes and certifications

Ways Rigur is supplied — form, process route, surface or paperwork — without a datasheet of their own. The property values above apply.

OptionWhat it isType
MATTE
Matte print stateSurface finish

What is Rigur?

Rigur (RGD450) is a polypropylene-simulating PolyJet photopolymer and the tougher, more impact-resistant successor to Durus, available in glossy, matte and digital-material blends. It is used for snap-fit and living-hinge prototypes that must survive repeated assembly cycles; default values are 42 MPa tensile strength, 32% elongation and Shore D 80. As a thermoset it cannot be melt-welded, it softens above about 45 °C, and daylight exposure requires a UV-blocking coating. Durus (RGD430) is the softer, lower-strength predecessor. Rigur has a density of 1.17 g/cm³ (0.0423 lb/in³), lighter than 54% of polymer grades. Its glass-transition temperature is 48°C (118 °F). Rigur has a yield strength of 38 MPa (5.51 ksi) and a tensile strength of 42 MPa (6.09 ksi) — weaker than 64% of polymer grades. Elongation at break is 32% and the elastic modulus is 1.9 GPa (0.276 Msi).

What is Rigur used for?

  • snap-fit closures
  • living hinges
  • sports equipment mockups

Limitations

  • Limited service temperature — 40°C (104 °F), worse than 99% of polymer grades
  • Difficult to weld — 5/100, worse than 89% of polymer grades
  • Degrades in UV without stabilisers — 20/100, worse than 88% of polymer grades
  • Absorbs moisture — dry before molding — 1.3%, worse than 88% of polymer grades
  • Limited formability — 15/100, worse than 79% of polymer grades

Rigur properties

Typical room-temperature values for Rigur-RGD450; bars are the position among polymer grades.

Physical3

Rigur has a density of 1.17 g/cm³ (0.0423 lb/in³), lighter than 54% of polymer grades. Its glass-transition temperature is 48°C (118 °F).

Density1.17 g/cm³0.04 lb/in³
Glass Transition (Tg)48°C118 °F
Water Absorption (24 h)1.3%

Mechanical16

Rigur has a yield strength of 38 MPa (5.51 ksi) and a tensile strength of 42 MPa (6.09 ksi) — weaker than 64% of polymer grades. Elongation at break is 32% and the elastic modulus is 1.9 GPa (0.276 Msi).

Elastic (Young's) Modulus1.9 GPa0.28 Msi
Poisson's Ratio0.4
Tensile Strength (Ultimate)42 MPa6.1 ksi
Yield Strength (0.2% offset)38 MPa5.5 ksi
Elongation at Break32%
Compressive Strength60 MPa8.7 ksi
Flexural Strength56 MPa8.1 ksi
Flexural Modulus1.4 GPa0.2 Msi
Shear Strength30 MPa4.4 ksi
Fracture Toughness (K_IC)2 MPa·√m1.8 ksi·√in
Izod Impact, Notched45 J/m0.84 ft·lbf/in
Hardness, Shore A95 Shore A
Hardness, Shore D80 Shore D
Hardness, Rockwell M55 HRM
Hardness, Rockwell R100 HRR
Tear Strength50 kN/m286 lbf/in

Thermal10

Rigur is rated for continuous service to 40°C (104 °F). It conducts heat at 0.2 W/m·K (0.116 BTU/hr·ft·°F), worse than 56% of polymer grades. Thermal expansion is 80 µm/m·K (44.4 µin/in·°F).

Thermal Conductivity0.2 W/m·K0.12 BTU/hr·ft·°F
Specific Heat Capacity1,500 J/kg·K0.36 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)80 µm/m·K44.4 µin/in·°F
Max Service Temperature (continuous)40°C104 °F
Min Service Temperature-20°C-4 °F
Heat Deflection Temp. @ 0.45 MPa47°C117 °F
Heat Deflection Temp. @ 1.8 MPa42°C107 °F
Vicat Softening Point (B50)50°C122 °F
Flammability (UL 94)Not UL 94 rated; treat as HB-class combustible acrylic photopolymer
Limiting Oxygen Index19%

Electrical4

Rigur is an electrical insulator with a dielectric strength of 18 kV/mm (457.2 V/mil) and a resistivity of 1×10¹³ Ω·m.

Electrical Resistivity1×10¹³ Ω·m3.94×10²⁰ µΩ·in
Dielectric Strength18 kV/mm457 V/mil
Dielectric Constant (1 MHz)3.2
Volume Resistivity1×10¹⁵ Ω·cm

Chemical & Environmental3

Corrosion resistance is very good (70/100), worse than 78% of polymer grades. UV resistance is poor.

Corrosion ResistanceVery good70/100
UV / Weathering ResistancePoor20/100
Chemical Resistance SummaryGood against water, dilute salts and weak acids/bases; swollen or attacked by alcohols, ketones, esters and chlorinated solvents; absorbs moisture (~1.3 %) with loss of stiffness; requires clear-coat or paint for any UV/outdoor exposure.

Sustainability3

Producing a kilogram of Rigur takes about 120 MJ of energy and emits 6.5 kg of CO₂ — more than 73% of polymer grades. Typical recycled content is 0%.

Embodied Energy (primary production)120 MJ/kg51,591 BTU/lb
Embodied Carbon (primary production)6.5 kg CO₂/kg
Typical Recycled Content0%

Manufacturability4

Rigur's machinability is fair (45/100, worse than 78% of polymer grades); weldability not recommended (5/100); formability poor (15/100).

MachinabilityFair45/100
WeldabilityNot recommended5/100
Formability (cold)Poor15/100
PolishabilityGood55/100

Common Calculations5

Specific Strength (UTS / density)calculated36 kN·m/kg
Specific Stiffness (E / density)calculated1.6 MN·m/kg
Modulus of Resiliencecalculated380 kJ/m³
Thermal Diffusivitycalculated0.1 mm²/s
Thermal Shock Resistance Indexcalculated0

Values are nominal handbook figures for design screening. Certified mill or lot data ships with every FabDigit order on request.

Strength versus weight in the polymer family

Yield strength against density for every polymer grade FabDigit runs. Rigur is highlighted; hover a dot for its name, or open the interactive family chart.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleRigur

Working with Rigur

Is Rigur easy to machine?

Drilling, tapping and sanding are fine at low speed; keep tooling cool since the part softens above ~45 °C.

Can Rigur be welded?

Thermoset — no melt welding; join with cyanoacrylate, epoxy or UV-cure acrylate adhesive.

Can Rigur be formed, bent or molded?

Built only by PolyJet jetting/UV cure; wall thickness ≥1 mm, and design living hinges thin (0.5–0.8 mm) with the hinge axis in the print plane.

Rigur chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
urethane acrylate oligomertoughening backbone15 – 3525
isobornyl acrylate10 – 2515
epoxy acrylate5 – 1510
inorganic filler / pigment (TiO2)white opacity, stiffness1 – 105
photoinitiatorUV cure package0.5 – 31.5
acrylic monomer blendreactive diluents≥ 25 (balance)

What surface finishes work on Rigur?

Water-jet or caustic bath support removal, then sand and prime; always apply UV-blocking clear coat or paint for parts kept in daylight.

Equivalent designations

Standards and trade names that resolve to Rigur in FabDigit's catalog. Equivalence is nominal — check the exact specification when certification matters.

Trade names
RGD450

How much does Rigur cost?

Rigur is a high-cost polymer ($$$$), pricier than about 78% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

Rigur — frequently asked

What is Rigur used for?

Rigur is typically used for snap-fit closures, living hinges and sports equipment mockups. In short: tougher polypropylene simulant; best snap-fit PolyJet resin; higher strength than Durus.

What is the yield strength of Rigur?

Rigur has a typical yield strength of 38 MPa (5.51 ksi) and a tensile strength of 42 MPa (6.09 ksi) — weaker than 64% of polymer grades. Strength varies by condition: see the 3 listed tempers.

Is Rigur easy to machine?

Reasonably — machinability is rated fair (45/100, worse than 78% of polymer grades). Drilling, tapping and sanding are fine at low speed; keep tooling cool since the part softens above ~45 °C.

Can Rigur be welded?

Not readily — weldability is rated not recommended (5/100). Thermoset — no melt welding; join with cyanoacrylate, epoxy or UV-cure acrylate adhesive.

What surface finishes work on Rigur?

Water-jet or caustic bath support removal, then sand and prime; always apply UV-blocking clear coat or paint for parts kept in daylight.

Can Rigur be formed, bent or molded?

Built only by PolyJet jetting/UV cure; wall thickness ≥1 mm, and design living hinges thin (0.5–0.8 mm) with the hinge axis in the print plane.

What is the maximum service temperature of Rigur?

Rigur is rated for continuous use to about 40°C (104 °F). Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

What is the difference between Rigur RGD450 and Rigur GLOSSY?

RGD450 is the default condition — default white Rigur cartridge printed on Objet/Connex PolyJet systems for PP-like functional prototypes. GLOSSY: choose when smooth, near-molded surface finish and slightly higher measured strength on skin surfaces are wanted. Yield strength is 38 MPa in RGD450 versus 40 MPa in GLOSSY.

How much does Rigur cost?

Rigur is a high-cost polymer ($$$$), pricier than about 78% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

Sources

  1. PolyJet Materials Data Sheet — Rigur RGD450 — Stratasys (2020)
  2. Rigur RGD450 Safety Data Sheet — Stratasys (2019)
  3. ASTM D638 / D790 / D256 / D648 test methods — ASTM International (2022)
  4. PolyJet (2025)

Property data is compiled from published supplier and standards handbooks and normalised for comparison; hardness values on non-Brinell scales are converted approximately for charting only. Manufacturability limits are FabDigit quote-engine defaults and may be relaxed by engineering review. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.