FabDigitFabDigit

TPU ESD

Grade

also Elastollan, Pellethane

ESD = eSD / antistatic conductive TPU

Use for antistatic hoses, conveyor parts and ESD-safe flexible components in electronics handling.

Values for the ESD condition

Other TPU grades and fills

TPU is listed in 19 conditions; see the grade overview at TPU.

Compare all 19 grades and fillsHide
Grade · open for datasheetBest forYield MPaTensile MPaElong. %Hardness
SLS powder
——413670 Shore A
SLS powder
——725086 Shore A
Formlabs TPU 90A Powder · SLS powder
A tough, skin-safe TPU elastomer for flexible parts requiring high elongation, tear resistance, and everyday durability.—931090 Shore A
MJF powder
A rubber-like TPU combining elasticity, rebound, fatigue resistance, and shock absorption for durable flexible parts.—928088 Shore A
SLS powder
——1031879 Shore A
MJF powder
A soft, durable TPU for complex flexible production parts and lattice structures with straightforward cold unpacking.—1544088 Shore A
MJF powder
A durable polyether TPU with high elasticity, abrasion resistance, energy rebound, and skin-contact suitability.—1740093 Shore A
Rigid engineering TPU
Choose for stiff snap-fit housings, wheel cores, chain guides and cable strain relief that must still absorb impact at low temperature.255532060 Shore D
FDM/FFF printed TPU filament (typ. 95A)
Use for printed flexible prototypes, gaskets and shoe midsoles; expect 60–80 % of injection-moulded strength and Z-direction weakness.—2838045 Shore D
Soft TPU
Pick for soft-touch overmoulds, flexible tubing, bellows and low-durometer seals.—2868070 Shore A
Halogen-free flame-retardant TPU
Specify for cable jackets, connectors and enclosures needing UL 94 V-0 at 1.5–3 mm; some loss of tear strength and elongation.—2840040 Shore D
ESDThis page
ESD / antistatic conductive TPU
Use for antistatic hoses, conveyor parts and ESD-safe flexible components in electronics handling.—3035042 Shore D
Aliphatic (HDI/H12MDI) optically clear, non-yellowing TPU
Use for clear films, paint-protection film, safety-glass interlayers and light guides where non-yellowing UV stability is required.—3550035 Shore D
Polyether-based TPU
Choose for wet, humid or microbe-exposed service and for good low-temperature flexibility; slightly lower abrasion/oil performance than ester.—3860034 Shore D
Shore A 85Default
Medium-soft general purpose TPU
Default all-round hardness for seals, cable jackets, wheels, grips and flexible parts.—4055033 Shore D
Shore A 60
Use when the design tolerates any TPU hardness and the exact grade is chosen later by the moulder.—4050040 Shore D
Polyester-based TPU
Best abrasion, tear, oil and fuel resistance at lowest cost — avoid continuous hot/humid or immersed service (hydrolysis).—4552038 Shore D
20 % glass-fibre reinforced TPU
Use where a semi-rigid, dimensionally stable structural part with TPU toughness is needed (housings, wheel hubs, sports hardware).—452570 Shore D
Hard elastomeric TPU
Pick for load-bearing rollers, couplings, ski boots, hose and abrasion-critical parts needing stiffness with flexibility.—5048045 Shore D

What is TPU ESD?

TPU ESD is TPU in the ESD grade — use for antistatic hoses, conveyor parts and ESD-safe flexible components in electronics handling. TPU ESD has a tensile strength of 30 MPa (4.35 ksi), weaker than 62% of polymer grades. Elongation at break is 350% and the elastic modulus is 0.06 GPa (0.0087 Msi). TPU ESD has a density of 1.18 g/cm³ (0.0426 lb/in³), heavier than 50% of polymer grades. Its glass-transition temperature is -40°C (-40 °F). Shore A 85 is the default condition FabDigit quotes; ESD is available on request or by drawing note.

Advantages

  • Ductile — tolerates forming and impact — 350%, better than 84% of polymer grades
  • Readily welded — 78/100, better than 84% of polymer grades
  • Conducts heat well — 0.26 W/m·K (0.15 BTU/hr·ft·°F), better than 77% of polymer grades
  • Forms and bends easily — 82/100, better than 77% of polymer grades

Limitations

  • Difficult to machine — 28/100, worse than 90% of polymer grades
  • Absorbs moisture — dry before molding — 0.8%, worse than 80% of polymer grades

TPU ESD properties

Typical room-temperature values for TPU ESD; 21 are specific to this condition. Other listed values are TPU reference data and may not represent this condition. Bars are the position among polymer grades.

Physical6

TPU ESD has a density of 1.18 g/cm³ (0.0426 lb/in³), heavier than 50% of polymer grades. Its glass-transition temperature is -40°C (-40 °F).

Density1.18 g/cm³0.04 lb/in³
Melting Temperature (Tm)185°C365 °F
Glass Transition (Tg)-40°C-40 °F
Water Absorption (24 h)0.8%
Water Absorption (Saturation)1.8%
Refractive Index1.51

Mechanical8

TPU ESD has a tensile strength of 30 MPa (4.35 ksi), weaker than 62% of polymer grades. Elongation at break is 350% and the elastic modulus is 0.06 GPa (0.0087 Msi).

Elastic (Young's) Modulus0.06 GPa0.01 Msi
Poisson's Ratio0.48
Tensile Strength (Ultimate)30 MPa4.4 ksi
Elongation at Break350%
Hardness, Shore A90 Shore A
Hardness, Shore D42 Shore D
Tear Strength50 kN/m286 lbf/in
Compression Set (22 h, 70 °C)42%

Thermal9

TPU ESD is rated for continuous service to 80°C (176 °F). It conducts heat at 0.26 W/m·K (0.15 BTU/hr·ft·°F), better than 77% of polymer grades. Thermal expansion is 170 µm/m·K (94.4 µin/in·°F).

Thermal Conductivity0.26 W/m·K0.15 BTU/hr·ft·°F
Specific Heat Capacity1,700 J/kg·K0.41 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)170 µm/m·K94.4 µin/in·°F
Max Service Temperature (continuous)80°C176 °F
Min Service Temperature-40°C-40 °F
Vicat Softening Point (B50)75°C167 °F
Flammability (UL 94)HB (standard non-FR grades, 1.5–3.0 mm)
Limiting Oxygen Index23%
Max Service Temperature (short-term)120°C248 °F

Electrical7

TPU ESD is an electrical insulator with a dielectric strength of 25 kV/mm (635 V/mil) and a resistivity of 100,000 Ω·m.

Electrical Resistivity100,000 Ω·m3.94×10¹² µΩ·in
Dielectric Strength25 kV/mm635 V/mil
Dielectric Constant (1 MHz)5
Dissipation Factor (1 MHz)0.05
Volume Resistivity1×10⁷ Ω·cm
Surface Resistivity1×10⁷ Ω
Comparative Tracking Index (CTI)600 V

Chemical & Environmental3

Corrosion resistance is very good (75/100), worse than 66% of polymer grades. UV resistance is fair.

Corrosion ResistanceVery good75/100
UV / Weathering ResistanceFair40/100
Chemical Resistance SummaryGood against mineral oils, greases, fuels and aliphatic solvents; polyester grades excel in oil/abrasion but hydrolyse above ~50 °C in humid service, polyether grades resist hydrolysis, microbes and low temperature. Attacked by strong acids/alkalis, ketones, esters, THF, DMF and chlorinated solvents; swells in hot polar solvents.

Sustainability4

Producing a kilogram of TPU ESD takes about 105 MJ of energy and emits 5.2 kg of CO₂ — more than 54% of polymer grades. Typical recycled content is 2%.

Embodied Energy (primary production)105 MJ/kg45,142 BTU/lb
Embodied Carbon (primary production)5.2 kg CO₂/kg
Embodied Water250 L/kg30 gal/lb
Typical Recycled Content2%

Manufacturability8

TPU ESD's machinability is poor (28/100, worse than 90% of polymer grades); weldability very good (78/100); formability very good (82/100).

MachinabilityPoor28/100
WeldabilityVery good78/100
Formability (cold)Very good82/100
PolishabilityFair40/100
Mold Shrinkage0.9%
Melt Flow Rate12 g/10 min
Processing Melt Temperature (typ.)210°C410 °F
Mold Temperature (typ.)30°C86 °F

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with TPU ESD

Is TPU easy to machine?

Machinable but gummy — use very sharp single-flute or polished carbide tools, high speed with low feed, air blast or chilling; harder D-grades cut far better than soft A-grades.

Can TPU be welded?

Readily joined by hot-air, hot-plate, ultrasonic, RF/high-frequency and laser welding; also solvent bondable with THF/DMF and cyanoacrylate/PU adhesives.

Can TPU be formed, bent or molded?

Dry pellets 2–4 h at 80–110 °C to <0.02 % moisture, melt 195–235 °C, mould 20–50 °C, generous gates and slow-then-fast fill; extrudes and thermoforms well, shrinkage 0.5–1.8 %.

What surface finishes work on TPU?

Takes flexible PU paints and pad/screen printing after flame or plasma pretreatment; not platable or polishable in the metal sense — surface texture is set by mould or print parameters.

TPU chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
MDI (4,4'-diphenylmethane diisocyanate) aromatic; HDI/H12MDI in aliphatic grades20 – 4530
1,4-butanediol chain extender4 – 128
processing aids / waxes / antioxidants0.2 – 20.8
glass fiberreinforced grades only0 – 300
flame retardant (halogen-free phosphorusFR V-0 grades only0 – 200
polyol soft segment (polyester adipate odefines ester vs ether family≥ 45 (balance)—

TPU ESD — frequently asked

What is TPU ESD used for?

TPU ESD is typically used for caster and skate wheels, hydraulic and pneumatic seals, drive and timing belts, cable jacketing and strain reliefs, protective phone and device cases and inflatable boat fabrics. In short: tough flexible elastic.

What is the tensile strength of TPU ESD?

TPU ESD has a typical tensile strength of 30 MPa (4.35 ksi) — weaker than 62% of polymer grades. Strength varies by condition: see the 19 listed tempers.

Is TPU ESD easy to machine?

Not especially — machinability is rated poor (28/100, worse than 90% of polymer grades). Machinable but gummy — use very sharp single-flute or polished carbide tools, high speed with low feed, air blast or chilling; harder D-grades cut far better than soft A-grades.

Can TPU ESD be welded?

Yes — weldability is rated very good (78/100). Readily joined by hot-air, hot-plate, ultrasonic, RF/high-frequency and laser welding; also solvent bondable with THF/DMF and cyanoacrylate/PU adhesives.

What surface finishes work on TPU ESD?

Takes flexible PU paints and pad/screen printing after flame or plasma pretreatment; not platable or polishable in the metal sense — surface texture is set by mould or print parameters.

Can TPU ESD be formed, bent or molded?

Dry pellets 2–4 h at 80–110 °C to <0.02 % moisture, melt 195–235 °C, mould 20–50 °C, generous gates and slow-then-fast fill; extrudes and thermoforms well, shrinkage 0.5–1.8 %.

What is the maximum service temperature of TPU ESD?

TPU ESD is rated for continuous use to about 80°C (176 °F), and briefly to 120°C. Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

Can FabDigit make parts in TPU ESD?

Yes — TPU ESD is available for CNC machining, sheet metal, injection molding and 3D printing; every part is priced by an engineer rather than instantly. Upload a STEP file to get a price and a DFM check.

Sources

  1. Elastollan Material Properties (TPU) brochure — BASF Polyurethanes (2023)
  2. Pellethane TPU product selection guide — Lubrizol Engineered Polymers (2022)
  3. Texin / Desmopan TPU datasheets — Covestro (2023)
  4. CAMPUS plastics database — TPU (ISO 10350 datasheets) — CAMPUS Consortium (2024)
  5. Sinterit Flexa Gray — Technical Data Sheet — Sinterit (2023)
  6. ISO 868 / ISO 37 / ISO 34-1 / ISO 815 elastomer test methods — ISO (2019)
  7. Lubrizol ESTANE 3D TPU M88A — Technical Data Sheet — Lubrizol (2023)
  8. Sinterit Flexa Bright — Technical Data Sheet — Sinterit (2022)
  9. EOS TPU 1301 — Technical Data Sheet — EOS
  10. Formlabs TPU 90A Powder — Technical Data Sheet — Formlabs (2023)
  11. Forward AM Ultrasint TPU01 — Technical Data Sheet — Forward AM (2021)
  12. Lubrizol ESTANE 3D TPU M95A — Technical Data Sheet — Lubrizol (2021)
  13. Engineered Materials Handbook Vol. 2: Engineering Plastics — ASM International (1988)

Property data is compiled from published supplier and standards handbooks and normalised for comparison. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.