FabDigit

Steel H21 Q&T (Quenched and tempered)

Heat-treated state

AISI/SAE H21 · UNS T20821 · EN 1.2581 · GB 3Cr2W8V

General hardened-and-tempered service condition for hot dies at 45–52 HRC.

CNC machiningStandard cost $$

Values for the Q&T condition

Other H21 tempers and conditions

H21 is listed in 7 conditions; see the grade overview at H21.

Compare all 7 conditionsHide
Condition · open for datasheetBest forYield MPaTensile MPaElong. %HardnessConductivity
AnnealedDefault
soft-annealed, as-supplied bar/plate
Standard stock condition for machining dies and inserts before hardening.6209001819 HRC3.1 % IACS
Hot Rolled / As-forged (unannealed)
Mill condition of large forged blocks before soft annealing; only for re-heat-treatment, not for machining.8501,1001034 HRC27 W/m·K
High-temper condition for maximum toughness
Pick for large hot-forging dies and dummy blocks where gross cracking, not wear, is the failure mode.1,1001,3001240 HRC28 W/m·K
Balanced hot-work die hardness
Most common working hardness for hot extrusion dies, punches and brass die-casting inserts.1,3501,600946 HRC28 W/m·K
Q&TThis page
Quenched and tempered
General hardened-and-tempered service condition for hot dies at 45–52 HRC.1,4501,700849 HRC—
hardened, tempered and gas/plasma nitrided surface
Surface treatment applied to finished dies to raise wear and washout resistance; core properties as Q&T.1,4501,700749 HRC28 W/m·K
High hardness for maximum hot wear resistance
Choose for hot shear blades and small punches where abrasive hot wear dominates and shock is low.1,6001,850552 HRC28 W/m·K

What is H21 Q&T?

H21 Q&T is H21 heat treated to Q&T — general hardened-and-tempered service condition for hot dies at 45–52 HRC. H21 Q&T has a yield strength of 1,450 MPa (210 ksi) and a tensile strength of 1,700 MPa (247 ksi) — stronger than 97% of steel grades. Elongation at break is 8% and the elastic modulus is 210 GPa (30.5 Msi). H21 Q&T has a density of 8.28 g/cm³ (0.299 lb/in³), heavier than 98% of steel grades. It melts at 1,420°C (2,588 °F). Annealed is the default condition FabDigit quotes; Q&T is available on request or by drawing note.

Advantages

  • High service temperature — 600°C (1,112 °F), better than 98% of steel grades
  • High strength — 1,450 MPa (210 ksi), better than 97% of steel grades
  • Polishes to a fine finish — 65/100, better than 78% of steel grades

Limitations

  • Low fracture toughness — 24 MPa·√m (21.8 ksi·√in), worse than 98% of steel grades
  • Difficult to machine — 15/100, worse than 98% of steel grades
  • Limited ductility — 8%, worse than 95% of steel grades
  • High embodied carbon — 3 kg CO₂/kg, worse than 91% of steel grades
  • Low electrical conductivity — 3.1 % IACS, worse than 89% of steel grades

H21 Q&T properties

Typical room-temperature values for H21 Q&T; 14 are specific to this condition. Other listed values are H21 reference data and may not represent this condition. Bars are the position among steel grades.

Physical3

H21 Q&T has a density of 8.28 g/cm³ (0.299 lb/in³), heavier than 98% of steel grades. It melts at 1,420°C (2,588 °F).

Density8.28 g/cm³0.3 lb/in³
Melting Point (Solidus)1,420°C2,588 °F
Liquidus Temperature1,480°C2,696 °F

Mechanical17

H21 Q&T has a yield strength of 1,450 MPa (210 ksi) and a tensile strength of 1,700 MPa (247 ksi) — stronger than 97% of steel grades. Elongation at break is 8% and the elastic modulus is 210 GPa (30.5 Msi).

Elastic (Young's) Modulus210 GPa30.5 Msi
Shear Modulus81 GPa11.7 Msi
Bulk Modulus160 GPa23.2 Msi
Poisson's Ratio0.29
Tensile Strength (Ultimate)1,700 MPa247 ksi
Yield Strength (0.2% offset)1,450 MPa210 ksi
Elongation at Break8%
Reduction in Area20%
Compressive Strength2,100 MPa305 ksi
Shear Strength1,050 MPa152 ksi
Fatigue Strength (Endurance Limit)700 MPa102 ksi
Fracture Toughness (K_IC)24 MPa·√m21.8 ksi·√in
Charpy V-Notch Impact (RT)10 J7.4 ft·lbf
Hardness, Brinell220 HB
Hardness, Rockwell B97 HRB
Hardness, Rockwell C49 HRC
Hardness, Vickers520 HV

Thermal6

H21 Q&T is rated for continuous service to 600°C (1,112 °F). It conducts heat at 27 W/m·K (15.6 BTU/hr·ft·°F), worse than 86% of steel grades. Thermal expansion is 11.8 µm/m·K (6.56 µin/in·°F).

Thermal Conductivity27 W/m·K15.6 BTU/hr·ft·°F
Specific Heat Capacity460 J/kg·K0.11 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)11.8 µm/m·K6.6 µin/in·°F
Latent Heat of Fusion250 J/g107 BTU/lb
Max Service Temperature (continuous)600°C1,112 °F
Min Service Temperature-20°C-4 °F

Electrical3

H21 Q&T conducts electricity at 3.1 % IACS, worse than 89% of steel grades.

Electrical Conductivity3.1 % IACS
Electrical Resistivity5.5×10⁻⁷ Ω·m21.7 µΩ·in
Magnetic Responseferromagnetic

Chemical & Environmental2

Corrosion resistance is poor (15/100), better than 75% of steel grades.

Corrosion ResistancePoor15/100
Chemical Resistance SummaryNo practical corrosion resistance: rusts in humid air and water, attacked by acids; requires oiling, phosphating or nitriding in service.

Sustainability4

Producing a kilogram of H21 Q&T takes about 42 MJ of energy and emits 3 kg of CO₂ — more than 92% of steel grades. Typical recycled content is 45%.

Embodied Energy (primary production)42 MJ/kg18,057 BTU/lb
Embodied Carbon (primary production)3 kg CO₂/kg
Embodied Water60 L/kg7.2 gal/lb
Typical Recycled Content45%

Manufacturability8

H21 Q&T's machinability is poor (15/100, worse than 98% of steel grades); weldability fair (35/100); formability poor (20/100).

MachinabilityPoor15/100
Machinability Rating (AISI 1212 = 100 %)15%
WeldabilityFair35/100
Formability (cold)Poor20/100
CastabilityPoor30/100
Brazeability / SolderabilityFair40/100
PolishabilityGood65/100
Anodizing Responsen/a — ferrous alloy; use nitriding, chromizing or oxide/phosphate coatings instead

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with H21 Q&T

Is H21 easy to machine?

Machine only in the annealed condition (≤241 HB) with rigid setups and coated carbide; tungsten carbides are abrasive so keep speeds moderate, and finish-grind after hardening.

Can H21 be welded?

Repair welding only: preheat 400–500 °C, matching W-alloy or H13-type filler, weld hot and temper immediately below the last tempering temperature to avoid cracking.

Can H21 be formed, bent or molded?

Hot work at 1050–1150 °C with slow furnace cooling and mandatory soft anneal (~870 °C, slow cool) afterwards; no meaningful cold formability.

What surface finishes work on H21?

Takes a good polish when hardened; protect with oiling, phosphate, nitriding or PVD/chromizing since bare surfaces rust and suffer hot washout.

H21 chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
C0.26 – 0.360.31
Si0.15 – 0.50.3
Mn0.15 – 0.40.3
Cr3 – 3.753.4
Wprimary hot-hardness element8.5 – 109.25
V0.3 – 0.60.45
Moresidual / optional≤ 0.5
Niresidual≤ 0.3
Curesidual≤ 0.25
P≤ 0.03
S≤ 0.03
Febalance

H21 Q&T — frequently asked

What is H21 Q&T used for?

H21 Q&T is typically used for brass and copper-alloy extrusion dies, hot punches and piercing points, hot forging die inserts, hot shear blades, extrusion mandrels and dummy blocks and die-casting dies for copper alloys. In short: hot-work tool steel.

What is the yield strength of H21 Q&T?

H21 Q&T has a typical yield strength of 1,450 MPa (210 ksi) and a tensile strength of 1,700 MPa (247 ksi) — stronger than 97% of steel grades. Strength varies by condition: see the 7 listed tempers.

Is H21 Q&T easy to machine?

Not especially — machinability is rated poor (15/100, worse than 98% of steel grades). Machine only in the annealed condition (≤241 HB) with rigid setups and coated carbide; tungsten carbides are abrasive so keep speeds moderate, and finish-grind after hardening.

Can H21 Q&T be welded?

With care — weldability is rated fair (35/100). Repair welding only: preheat 400–500 °C, matching W-alloy or H13-type filler, weld hot and temper immediately below the last tempering temperature to avoid cracking.

What surface finishes work on H21 Q&T?

Takes a good polish when hardened; protect with oiling, phosphate, nitriding or PVD/chromizing since bare surfaces rust and suffer hot washout.

Can H21 Q&T be formed, bent or molded?

Hot work at 1050–1150 °C with slow furnace cooling and mandatory soft anneal (~870 °C, slow cool) afterwards; no meaningful cold formability.

What is the maximum service temperature of H21 Q&T?

H21 Q&T is rated for continuous use to about 600°C (1,112 °F). Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

Can FabDigit make parts in H21 Q&T?

Yes — H21 Q&T is available for CNC machining; every part is priced by an engineer rather than instantly. Upload a STEP file to get a price and a DFM check.

Sources

  1. ASTM A681 – Standard Specification for Tool Steels Alloy — ASTM International (2015)
  2. GB/T 1299 (3Cr2W8V) — SAC (2014)
  3. ASM Handbook Vol.1 – Properties and Selection: Irons, Steels, and High-Performance Alloys (Tool Steels) — ASM International (1990)
  4. Tool Steels, 5th ed. (Roberts, Krauss, Kennedy) — ASM International (1998)
  5. X30WCrV9-3 / 1.2581 hot-work tool steel datasheet — Böhler / Ovako-class producers (2020)

Property data is compiled from published supplier and standards handbooks and normalised for comparison. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.