FabDigit

Steel F1-N (Normalized)

Heat-treated state

UNS T60601

Intermediate condition used to refine grain and homogenise forgings before spheroidize annealing; not a service condition.

Standard cost $$

Values for the N condition

Other F1 tempers and conditions

F1 is listed in 7 conditions; see the grade overview at F1.

Compare all 7 conditionsHide
Condition · open for datasheetBest forYield MPaTensile MPaElong. %HardnessConductivity
ANNDefault
Annealed
Standard stock condition for machining, sawing and shaping tool blanks before water hardening.42070020197 HB44 W/m·K
NThis page
Normalized
Intermediate condition used to refine grain and homogenise forgings before spheroidize annealing; not a service condition.5209001029 HRC9 % IACS
Cold Drawn Annealed
Pick for close-tolerance, bright-finish small bar used for taps, punches and pins with minimal pre-machining.6007801217 HRC9.5 % IACS
Carburized and hardened
Exploits the grade's low hardenability: hard wear-resistant skin ~1.5–4 mm deep over an unhardened tough core for impact tooling.1,0001,200262 HRC7.5 % IACS
Hardened & Tempered 260 °C
Highest-toughness hardened condition for shock-loaded light tooling; upper practical tempering limit for this grade.1,6001,900457 HRC—
Hardened & Tempered 205 °C
Balanced hardening condition for punches, dies, woodworking cutters and taps needing some shock resistance.1,7502,050260 HRC—
Hardened & Tempered 150 °C
Maximum hardness and wear resistance for paper/leather knives, engraving tools and light blanking punches; minimum toughness.1,9002,200163 HRC38 W/m·K

What is F1-N?

F1-N is F1 heat treated to N — intermediate condition used to refine grain and homogenise forgings before spheroidize annealing; not a service condition. F1-N has a yield strength of 520 MPa (75.4 ksi) and a tensile strength of 900 MPa (131 ksi) — stronger than 67% of steel grades. Elongation at break is 10% and the elastic modulus is 205 GPa (29.7 Msi). F1-N has a density of 7.8 g/cm³ (0.282 lb/in³), lighter than 87% of steel grades. It melts at 1,420°C (2,588 °F). ANN is the default condition FabDigit quotes; N is available on request or by drawing note.

Advantages

  • Polishes to a fine finish — 75/100, better than 94% of steel grades

Limitations

  • Difficult to weld — 10/100, worse than 99% of steel grades
  • Limited formability — 12/100, worse than 92% of steel grades
  • Limited ductility — 10%, worse than 91% of steel grades
  • Limited service temperature — 250°C (482 °F), worse than 85% of steel grades

F1-N properties

Typical room-temperature values for F1-N; 22 are specific to this condition. Other listed values are F1 reference data and may not represent this condition. Bars are the position among steel grades.

Physical3

F1-N has a density of 7.8 g/cm³ (0.282 lb/in³), lighter than 87% of steel grades. It melts at 1,420°C (2,588 °F).

Density7.8 g/cm³0.28 lb/in³
Melting Point (Solidus)1,420°C2,588 °F
Liquidus Temperature1,470°C2,678 °F

Mechanical15

F1-N has a yield strength of 520 MPa (75.4 ksi) and a tensile strength of 900 MPa (131 ksi) — stronger than 67% of steel grades. Elongation at break is 10% and the elastic modulus is 205 GPa (29.7 Msi).

Elastic (Young's) Modulus205 GPa29.7 Msi
Shear Modulus80 GPa11.6 Msi
Bulk Modulus160 GPa23.2 Msi
Poisson's Ratio0.29
Tensile Strength (Ultimate)900 MPa131 ksi
Yield Strength (0.2% offset)520 MPa75.4 ksi
Elongation at Break10%
Reduction in Area28%
Compressive Strength540 MPa78.3 ksi
Shear Strength560 MPa81.2 ksi
Fatigue Strength (Endurance Limit)405 MPa58.7 ksi
Charpy V-Notch Impact (RT)12 J8.9 ft·lbf
Hardness, Brinell285 HB
Hardness, Rockwell B93 HRB
Hardness, Vickers300 HV

Thermal6

F1-N is rated for continuous service to 250°C (482 °F). It conducts heat at 40 W/m·K (23.1 BTU/hr·ft·°F), worse than 64% of steel grades. Thermal expansion is 11.5 µm/m·K (6.39 µin/in·°F).

Thermal Conductivity40 W/m·K23.1 BTU/hr·ft·°F
Specific Heat Capacity460 J/kg·K0.11 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)11.5 µm/m·K6.4 µin/in·°F
Latent Heat of Fusion250 J/g107 BTU/lb
Max Service Temperature (continuous)250°C482 °F
Min Service Temperature-30°C-22 °F

Electrical3

F1-N conducts electricity at 9 % IACS, better than 71% of steel grades.

Electrical Conductivity9 % IACS
Electrical Resistivity1.9×10⁻⁷ Ω·m7.48 µΩ·in
Magnetic Responseferromagnetic

Chemical & Environmental3

Corrosion resistance is not recommended (10/100), worse than 86% of steel grades.

Galvanic Potential (seawater, vs SCE)-0.6 V
Corrosion ResistanceNot recommended10/100
Chemical Resistance SummaryNo inherent corrosion resistance: rusts in humid air and any aqueous/acid media; requires oiling, phosphating or plating. Resists dry hydrocarbons, oils and greases.

Sustainability4

Producing a kilogram of F1-N takes about 33 MJ of energy and emits 2.3 kg of CO₂ — more than 76% of steel grades. Typical recycled content is 30%.

Embodied Energy (primary production)33 MJ/kg14,187 BTU/lb
Embodied Carbon (primary production)2.3 kg CO₂/kg
Embodied Water60 L/kg7.2 gal/lb
Typical Recycled Content30%

Manufacturability8

F1-N's machinability is fair (42/100, worse than 73% of steel grades); weldability not recommended (10/100); formability not recommended (12/100).

MachinabilityFair42/100
Machinability Rating (AISI 1212 = 100 %)55%
WeldabilityNot recommended10/100
Formability (cold)Not recommended12/100
CastabilityPoor25/100
Brazeability / SolderabilityFair45/100
PolishabilityVery good75/100
Anodizing Responsen/a — ferrous alloy; use blackening, phosphating or hard chrome instead

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with F1-N

Is F1 easy to machine?

Machine only in the spheroidize-annealed condition (~75 % of AISI 1212) with sharp HSS/carbide and steady feeds; after water hardening it must be ground with soft, free-cutting wheels and ample coolant to avoid grinding cracks.

Can F1 be welded?

Essentially non-weldable for structural joints; repair only with preheat 300–400 °C, matched high-carbon filler, immediate stress relief and re-hardening — cracking and soft zones are otherwise certain.

Can F1 be formed, bent or molded?

Hot forge 1010→860 °C then slow cool and spheroidize anneal at 760–790 °C; cold forming limited to mild bending of annealed strip. Harden from 790–845 °C with brine/water quench (allow ~1.5–4 mm case) and temper immediately at 150–260 °C — never above 260 °C.

What surface finishes work on F1?

Takes a fine polish for cutting edges; provide corrosion protection by oiling, black oxide, phosphate or thin hard chrome — no anodizing, and any plating bake-out must stay below the tempering temperature.

F1 chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
CASTM A686 F10.95 – 1.251
Mn0.1 – 0.40.25
Si0.1 – 0.40.25
Wprincipal carbide former for wear resistance1 – 1.751.25
Croptional/residual≤ 0.30.15
Voptional/residual≤ 0.25
Moresidual≤ 0.25
Niresidual≤ 0.3
P≤ 0.03
S≤ 0.03
Febalance

F1-N — frequently asked

What is F1-N used for?

F1-N is typically used for taps, reamers, light punches, small dies and hand tools. In short: water-hardening tungsten grade; shallow case, tough core; best machinability of family.

What is the yield strength of F1-N?

F1-N has a typical yield strength of 520 MPa (75.4 ksi) and a tensile strength of 900 MPa (131 ksi) — stronger than 67% of steel grades. Strength varies by condition: see the 7 listed tempers.

Is F1-N easy to machine?

Not especially — machinability is rated fair (42/100, worse than 73% of steel grades). Machine only in the spheroidize-annealed condition (~75 % of AISI 1212) with sharp HSS/carbide and steady feeds; after water hardening it must be ground with soft, free-cutting wheels and ample coolant to avoid grinding cracks.

Can F1-N be welded?

Not readily — weldability is rated not recommended (10/100). Essentially non-weldable for structural joints; repair only with preheat 300–400 °C, matched high-carbon filler, immediate stress relief and re-hardening — cracking and soft zones are otherwise certain.

What surface finishes work on F1-N?

Takes a fine polish for cutting edges; provide corrosion protection by oiling, black oxide, phosphate or thin hard chrome — no anodizing, and any plating bake-out must stay below the tempering temperature.

Can F1-N be formed, bent or molded?

Hot forge 1010→860 °C then slow cool and spheroidize anneal at 760–790 °C; cold forming limited to mild bending of annealed strip. Harden from 790–845 °C with brine/water quench (allow ~1.5–4 mm case) and temper immediately at 150–260 °C — never above 260 °C.

What is the maximum service temperature of F1-N?

F1-N is rated for continuous use to about 250°C (482 °F). Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

What is the difference between F1-ANN and F1 HT-64?

ANN is the default condition — standard stock condition for machining, sawing and shaping tool blanks before water hardening. HT-64: maximum hardness and wear resistance for paper/leather knives, engraving tools and light blanking punches; minimum toughness. Yield strength is 420 MPa in ANN versus 1,900 MPa in HT-64.

Sources

  1. ASTM A686 — Standard Specification for Carbon Tool Steels — ASTM International (2019)
  2. ASM Handbook Vol.1: Properties and Selection — Irons, Steels, and High-Performance Alloys (Tool Steels) — ASM International (1990)
  3. Tool Steels, 5th ed. (Roberts, Krauss, Kennedy) — ASM International (1998)
  4. ASM Handbook Vol.16: Machining — ASM International (1989)
  5. SAE J437/J438 — Tool and Die Steels — SAE International (2015)

Property data is compiled from published supplier and standards handbooks and normalised for comparison. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.