FabDigitFabDigit

Silicone TC

Additive grade

also PDMS, LSR

TC = thermally conductive (alumina / boron nitride filled) silicone

Pick for thermal interface pads, gap fillers and potting where heat must be moved but electrical isolation kept.

Injection moldingPremium cost $$$

Values for the TC condition

Other Silicone grades and fills

Silicone is listed in 15 conditions; see the grade overview at Silicone.

Compare all 15 grades and fillsHide
Grade · open for datasheetBest forYield MPaTensile MPaElong. %Hardness
Sponge/Foam
Pick for low-closure-force weather seals, cushioning and insulation in enclosures and ovens.—215025 Shore A
Electrically conductive silicone
Pick for EMI gaskets, grounding pads and ESD-safe seals combining shielding with environmental sealing.—312020 Shore D
TCThis page
Thermally conductive (alumina / boron nitride filled) silicone
Pick for thermal interface pads, gap fillers and potting where heat must be moved but electrical isolation kept.—312018 Shore D
RTV-2 / Cast PDMS
Pick for prototyping molds, microfluidic PDMS chips, potting and encapsulation where no heated press is available.—63508 Shore D
soft grade
Pick for soft-touch skins, low-force seals, membranes and conformal cushions.—76506 Shore D
heat-stabilized (iron oxide / rare-earth) silicone, 250–300 °C capable
Pick for oven gaskets, exhaust/turbo seals, ironing and heater components where continuous service exceeds 200 °C.—735015 Shore D
flame-retardant silicone (UL 94 V-0)
Pick for rail, EV battery and appliance parts needing UL 94 V-0 with low smoke and halogen-free formulation.—735016 Shore D
soft-medium grade
Pick for baby-care parts, low-compression-force gaskets and flexible tubing.—85509 Shore D
HCR/HTV
Pick for extruded profiles, tubing, calendered sheet and low-volume compression-molded gaskets.—840015 Shore D
Fluorosilicone, fuel and oil resistant
Pick when silicone-level cold flexibility is needed together with resistance to fuels, hydrocarbon oils and solvents.—825016 Shore D
general purpose grade
Pick as the default all-round hardness for O-rings, keypads and static seals.—945012 Shore D
Liquid silicone rubber, 2-part platinum cure, injection molded
Pick for high-volume automated injection molding of thin, flash-free, dimensionally precise parts.—955012 Shore D
medium-hard grade
Pick for dynamic seals, grommets and parts needing better set resistance and extrusion resistance.—940015 Shore D
extra-hard grade
Pick for rollers, back-up rings and parts resisting extrusion under high clamp loads.—922030 Shore D
hard grade
Pick for high-pressure gaskets, valve seats and stiff overmolds.—1032022 Shore D

What is Silicone TC?

Silicone TC is Silicone in the TC grade — pick for thermal interface pads, gap fillers and potting where heat must be moved but electrical isolation kept. Silicone TC has a tensile strength of 3 MPa (0.435 ksi), weaker than 83% of polymer grades. Elongation at break is 120% and the elastic modulus is 0.01 GPa (8.7×10⁻⁴ Msi). Silicone TC has a density of 2.3 g/cm³ (0.0831 lb/in³), heavier than 100% of polymer grades. Its glass-transition temperature is -125°C (-193 °F).

Advantages

  • Conducts heat well — 1.5 W/m·K (0.867 BTU/hr·ft·°F), better than 100% of polymer grades
  • Good UV / weathering resistance — 97/100, better than 98% of polymer grades
  • Polishes to a fine finish — 85/100, better than 92% of polymer grades
  • High service temperature — 200°C (392 °F), better than 87% of polymer grades

Limitations

  • Heavy — 2.3 g/cm³ (0.0831 lb/in³), worse than 100% of polymer grades
  • Difficult to machine — 25/100, worse than 93% of polymer grades
  • Low stiffness — 0.01 GPa (8.7×10⁻⁴ Msi), worse than 86% of polymer grades

Silicone TC properties

Typical room-temperature values for Silicone TC; 18 are specific to this condition. Other listed values are Silicone reference data and may not represent this condition. Bars are the position among polymer grades.

Physical5

Silicone TC has a density of 2.3 g/cm³ (0.0831 lb/in³), heavier than 100% of polymer grades. Its glass-transition temperature is -125°C (-193 °F).

Density2.3 g/cm³0.08 lb/in³
Glass Transition (Tg)-125°C-193 °F
Water Absorption (24 h)0.3%
Refractive Index1.41
Light Transmission88%

Mechanical9

Silicone TC has a tensile strength of 3 MPa (0.435 ksi), weaker than 83% of polymer grades. Elongation at break is 120% and the elastic modulus is 0.01 GPa (8.7×10⁻⁴ Msi).

Elastic (Young's) Modulus0.01 GPa8.7×10⁻⁴ Msi
Shear Modulus7.5×10⁻⁴ GPa1.09×10⁻⁴ Msi
Bulk Modulus2 GPa0.22 Msi
Poisson's Ratio0.49
Tensile Strength (Ultimate)3 MPa0.44 ksi
Elongation at Break120%
Hardness, Shore A60 Shore A
Tear Strength10 kN/m57.1 lbf/in
Compression Set (22 h, 70 °C)30%

Thermal8

Silicone TC is rated for continuous service to 200°C (392 °F). It conducts heat at 1.5 W/m·K (0.867 BTU/hr·ft·°F), better than 100% of polymer grades. Thermal expansion is 270 µm/m·K (150 µin/in·°F).

Thermal Conductivity1.5 W/m·K0.87 BTU/hr·ft·°F
Specific Heat Capacity1,300 J/kg·K0.31 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)270 µm/m·K150 µin/in·°F
Max Service Temperature (continuous)200°C392 °F
Min Service Temperature-60°C-76 °F
Flammability (UL 94)HB (unfilled); V-0 achievable with FR-filled compounds
Limiting Oxygen Index38%
Max Service Temperature (short-term)250°C482 °F

Electrical7

Silicone TC is an electrical insulator with a dielectric strength of 12 kV/mm (304.8 V/mil) and a resistivity of 1×10¹¹ Ω·m.

Electrical Resistivity1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
Dielectric Strength12 kV/mm305 V/mil
Dielectric Constant (1 MHz)3
Dissipation Factor (1 MHz)0.002
Volume Resistivity1×10¹³ Ω·cm
Surface Resistivity1×10¹⁴ Ω
Comparative Tracking Index (CTI)600 V

Chemical & Environmental3

Corrosion resistance is excellent (88/100), better than 74% of polymer grades. UV resistance is excellent.

Corrosion ResistanceExcellent88/100
UV / Weathering ResistanceExcellent97/100
Chemical Resistance SummaryExcellent vs water, steam (short), ozone, UV, dilute acids/alkalis, alcohols, many aqueous media and body fluids; poor vs concentrated acids, ketones, aromatic/chlorinated solvents, fuels and hot mineral oils (which cause large swell) — use fluorosilicone for fuel/oil.

Sustainability4

Producing a kilogram of Silicone TC takes about 110 MJ of energy and emits 6.5 kg of CO₂ — more than 64% of polymer grades. Typical recycled content is 0%.

Embodied Energy (primary production)110 MJ/kg47,292 BTU/lb
Embodied Carbon (primary production)6.5 kg CO₂/kg
Embodied Water250 L/kg30 gal/lb
Typical Recycled Content0%

Manufacturability7

Silicone TC's machinability is poor (25/100, worse than 93% of polymer grades); weldability poor (20/100); formability very good (70/100).

MachinabilityPoor25/100
WeldabilityPoor20/100
Formability (cold)Very good70/100
PolishabilityExcellent85/100
Mold Shrinkage1.5%
Processing Melt Temperature (typ.)25°C77 °F
Mold Temperature (typ.)180°C356 °F

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with Silicone TC

Is Silicone easy to machine?

Cured silicone is not conventionally machinable — use die cutting, waterjet, laser (with fume control) or cryogenic deflashing; sharp new blades and water lubrication prevent tearing.

Can Silicone be welded?

No thermal welding; join by uncured silicone adhesive, self-bonding primers, RTV, or oxygen-plasma bonding for PDMS microfluidics; secondary overmolding onto cured silicone requires primer.

Can Silicone be formed, bent or molded?

LSR: cold runner, 165–210 °C mold, 15–60 s cure, allow 2–3 % shrink and vacuum-vented tools; HCR: compression/transfer or extrusion + hot-air/steam cure; post-cure 200 °C/4 h to remove volatiles for medical/food use.

What surface finishes work on Silicone?

Surface finish is fully set by the mold (mirror EDM or texture); paints do not adhere without silicone-specific primer — use plasma/corona treatment, parylene or silicone inks; talc-free anti-block coatings for tack reduction.

Silicone chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
fumed silica (reinforcing filler)surface-treated, sets modulus and tear strength15 – 3525
hydride crosslinker (Si-H siloxane)addition-cure systems0.5 – 31.5
platinum catalyst (Karstedt)peroxide (DCBP/DBPMH) used instead in HCR peroxide cure2×10⁻⁴ – 05×10⁻⁴
extending filler / pigment / heat stabile.g. ground quartz, Fe2O3, Ce compounds0 – 155
polydimethylsiloxane (PDMS) base polymermay contain vinyl-methyl and phenyl or trifluoropropyl substitution≥ 55 (balance)—

Silicone TC — frequently asked

What is Silicone TC used for?

Silicone TC is typically used for O-rings and moulded gaskets, medical tubing and implant seals, keypads and button mats, baby bottle nipples and food-contact seals, electronic potting and encapsulation and high-temperature oven and appliance seals. In short: biocompatible soft silicone.

What is the tensile strength of Silicone TC?

Silicone TC has a typical tensile strength of 3 MPa (0.435 ksi) — weaker than 83% of polymer grades. Strength varies by condition: see the 15 listed tempers.

Is Silicone TC easy to machine?

Not especially — machinability is rated poor (25/100, worse than 93% of polymer grades). Cured silicone is not conventionally machinable — use die cutting, waterjet, laser (with fume control) or cryogenic deflashing; sharp new blades and water lubrication prevent tearing.

Can Silicone TC be welded?

Not readily — weldability is rated poor (20/100). No thermal welding; join by uncured silicone adhesive, self-bonding primers, RTV, or oxygen-plasma bonding for PDMS microfluidics; secondary overmolding onto cured silicone requires primer.

What surface finishes work on Silicone TC?

Surface finish is fully set by the mold (mirror EDM or texture); paints do not adhere without silicone-specific primer — use plasma/corona treatment, parylene or silicone inks; talc-free anti-block coatings for tack reduction.

Can Silicone TC be formed, bent or molded?

LSR: cold runner, 165–210 °C mold, 15–60 s cure, allow 2–3 % shrink and vacuum-vented tools; HCR: compression/transfer or extrusion + hot-air/steam cure; post-cure 200 °C/4 h to remove volatiles for medical/food use.

What is the maximum service temperature of Silicone TC?

Silicone TC is rated for continuous use to about 200°C (392 °F), and briefly to 250°C. Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

Can FabDigit make parts in Silicone TC?

Yes — Silicone TC is available for injection molding; every part is priced by an engineer rather than instantly. Upload a STEP file to get a price and a DFM check.

Sources

  1. ASTM D2000 — Classification System for Rubber Products (VMQ/FVMQ) — ASTM (2023)
  2. ASTM D412 / D624 / D395 / D2240 — tensile, tear, compression set, durometer — ASTM (2022)
  3. SILASTIC / Dow LSR and HCR product datasheets — Dow (2023)
  4. ELASTOSIL LR / R silicone rubber datasheets — Wacker Chemie (2023)
  5. Silopren LSR and thermally conductive silicone data — Momentive (2022)
  6. ASM Engineered Materials Handbook Vol. 2 — Engineering Plastics/Elastomers — ASM International (1988)
  7. CAMPUS / UL Prospector elastomer entries — UL / CAMPUS (2024)

Property data is compiled from published supplier and standards handbooks and normalised for comparison. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.