FabDigit

PTMT

Historical/alternate name for polybutylene terephthalate (the repeat unit's tetramethylene glycol segment); chemically identical resin to PBT, still seen in older electrical/electronics literature and some Asian datasheets.

Standard cost $$

Reference datasheet — PTMT is not in the instant-quote catalog. Upload your part and an engineer will quote it in this grade or suggest the closest stocked equivalent.

PTMT grades and fills

PTMT is supplied in 17 conditions, soft to hard.

Compare all 17 grades and fillsHide
Grade · open for datasheetBest forYield MPaTensile MPaElong. %Hardness
Impact-modified
Use where notched impact and cold-temperature toughness dominate — snap fits, handles, exterior clips.404220068 Shore D
PBT/ASA (or PBT/ABS) blend
Blend for weatherable, low-warp cosmetic housings needing better surface than glass-filled PBT.45454074 Shore D
PTFE / silicone lubricated bearing grade
Internally lubricated compound for gears, cams and slide bushings running dry against metal.47481578 Shore D
FR V-0 unfilled
For live-part enclosures and switch bodies needing V-0 at 0.75–1.5 mm without reinforcement.5015
PBT/PC blend
Alloy for tough, dimensionally stable painted exterior parts (bumper fascia, trims) with better impact than neat PBT.555512076 Shore D
Mineral-filled
Choose when flatness and isotropic shrinkage matter more than strength — flat covers, lids, painted parts.5860485 Shore D
ESD / conductive
For electronics trays, fuel-system parts and housings needing static dissipation (10^4–10^9 Ω/sq).70385 Shore D
10 % glass-fiber reinforced
Light stiffening with modest warpage penalty; used where the unfilled grade is just too soft.805
15 % glass-fiber reinforced
Balance of stiffness and low warpage for connector bodies and covers.954
Glass + mineral filled
Compromise grade: near-GF stiffness with much flatter parts for large thin covers and housings.95952.588 Shore D
20 % glass-fiber reinforced
Common automotive/electrical structural grade when GF30 warps too much.1103.5
flame-retardant, 30 % glass reinforced
Most-specified E&E grade: V-0 plus HDT > 200 °C for relay bases, breaker parts and connectors.1252.2
Hot rolled
Carbodiimide-stabilized grades for automotive connectors and pumps exposed to hot humid air or coolant mist.1302.586 Shore D
30 % glass-fiber reinforced
The standard reinforced PBT for connectors, bobbins, brackets and under-hood parts needing HDT > 200 °C.1352.890 HRM
40 % glass-fiber reinforced
Maximum stiffness/creep resistance for metal-replacement brackets; expect anisotropic shrink and abrasive wear on tooling.1502.2
50 % glass-fiber reinforced
Highest-modulus PBT compound for load-bearing housings; surface quality and toughness are the trade-off.1652
CF20/CF30
Pick for high stiffness at low weight plus static-dissipative surface; costlier and more anisotropic than glass.1751.8

Supply forms, finishes and certifications

Ways PTMT is supplied — form, process route, surface or paperwork — without a datasheet of their own. The property values above apply.

OptionWhat it isType
EXT
Extrusion / stock-shape gradeSupply form
FDA
Food-contact / FDA-compliant gradeCertification
UV
UV-stabilized / weatherableGrade option
UnfilledDefault
Unfilled / NaturalStandard supply

What is PTMT?

Historical/alternate name for polybutylene terephthalate (the repeat unit's tetramethylene glycol segment); chemically identical resin to PBT, still seen in older electrical/electronics literature and some Asian datasheets. PTMT has a density of 1.31 g/cm³ (0.0473 lb/in³), heavier than 71% of polymer grades. Its glass-transition temperature is 50°C (122 °F). PTMT has a yield strength of 55 MPa (7.98 ksi) and a tensile strength of 55 MPa (7.98 ksi) — stronger than 62% of polymer grades. Elongation at break is 100% and the elastic modulus is 2.6 GPa (0.377 Msi).

What is PTMT used for?

  • Electrical bobbins and connectors
  • Precision gears and bushings
  • Automotive electrical components
  • Consumer electronics parts

Advantages

  • Low moisture uptake — 0.08%, better than 80% of polymer grades

PTMT properties

Typical room-temperature values; bars are the position among polymer grades.

Physical6

PTMT has a density of 1.31 g/cm³ (0.0473 lb/in³), heavier than 71% of polymer grades. Its glass-transition temperature is 50°C (122 °F).

Density1.31 g/cm³0.05 lb/in³
Melting Temperature (Tm)225°C437 °F
Glass Transition (Tg)50°C122 °F
Water Absorption (24 h)0.08%
Water Absorption (Saturation)0.45%
Refractive Index1.58

Mechanical16

PTMT has a yield strength of 55 MPa (7.98 ksi) and a tensile strength of 55 MPa (7.98 ksi) — stronger than 62% of polymer grades. Elongation at break is 100% and the elastic modulus is 2.6 GPa (0.377 Msi).

Elastic (Young's) Modulus2.6 GPa0.38 Msi
Shear Modulus0.95 GPa0.14 Msi
Bulk Modulus4 GPa0.58 Msi
Poisson's Ratio0.4
Tensile Strength (Ultimate)55 MPa8 ksi
Yield Strength (0.2% offset)55 MPa8 ksi
Elongation at Break100%
Compressive Strength85 MPa12.3 ksi
Compressive Modulus2.4 GPa0.35 Msi
Flexural Strength88 MPa12.8 ksi
Flexural Modulus2.4 GPa0.35 Msi
Shear Strength45 MPa6.5 ksi
Izod Impact, Notched50 J/m0.94 ft·lbf/in
Hardness, Shore D82 Shore D
Hardness, Rockwell M70 HRM
Hardness, Rockwell R118 HRR

Thermal11

PTMT is rated for continuous service to 120°C (248 °F). It conducts heat at 0.23 W/m·K (0.133 BTU/hr·ft·°F), better than 65% of polymer grades. Thermal expansion is 80 µm/m·K (44.4 µin/in·°F).

Thermal Conductivity0.23 W/m·K0.13 BTU/hr·ft·°F
Specific Heat Capacity1,500 J/kg·K0.36 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)80 µm/m·K44.4 µin/in·°F
Max Service Temperature (continuous)120°C248 °F
Min Service Temperature-40°C-40 °F
Heat Deflection Temp. @ 0.45 MPa150°C302 °F
Heat Deflection Temp. @ 1.8 MPa60°C140 °F
Vicat Softening Point (B50)178°C352 °F
Flammability (UL 94)HB (unfilled natural resin, 0.8–3.0 mm); V-0 only with flame-retardant compounding
Limiting Oxygen Index21%
Max Service Temperature (short-term)160°C320 °F

Electrical7

PTMT is an electrical insulator with a dielectric strength of 22 kV/mm (558.8 V/mil) and a resistivity of 1×10¹⁴ Ω·m.

Electrical Resistivity1×10¹⁴ Ω·m3.94×10²¹ µΩ·in
Dielectric Strength22 kV/mm559 V/mil
Dielectric Constant (1 MHz)3.1
Dissipation Factor (1 MHz)0.018
Volume Resistivity1×10¹⁶ Ω·cm
Surface Resistivity1×10¹⁵ Ω
Comparative Tracking Index (CTI)600 V

Chemical & Environmental3

Corrosion resistance is very good (78/100), worse than 61% of polymer grades. UV resistance is fair.

Corrosion ResistanceVery good78/100
UV / Weathering ResistanceFair35/100
Chemical Resistance SummaryGood against fuels, mineral oils, greases, aliphatic hydrocarbons, alcohols, dilute acids and most salt solutions; attacked by strong alkalis, ammonia, phenols, hot chlorinated solvents; hydrolyses in hot water/steam above ~60 °C — use hydrolysis-stabilized grades for wet-heat service.

Sustainability4

Producing a kilogram of PTMT takes about 95 MJ of energy and emits 4.4 kg of CO₂ — less than 70% of polymer grades. Typical recycled content is 5%.

Embodied Energy (primary production)95 MJ/kg40,843 BTU/lb
Embodied Carbon (primary production)4.4 kg CO₂/kg
Embodied Water250 L/kg30 gal/lb
Typical Recycled Content5%

Manufacturability8

PTMT's machinability is good (68/100, better than 71% of polymer grades); weldability very good (70/100); formability poor (30/100).

MachinabilityGood68/100
WeldabilityVery good70/100
Formability (cold)Poor30/100
PolishabilityFair45/100
Mold Shrinkage1.7%
Melt Flow Rate25 g/10 min
Processing Melt Temperature (typ.)255°C491 °F
Mold Temperature (typ.)70°C158 °F

Common Calculations5

Specific Strength (UTS / density)calculated42 kN·m/kg
Specific Stiffness (E / density)calculated2 MN·m/kg
Modulus of Resiliencecalculated582 kJ/m³
Thermal Diffusivitycalculated0.1 mm²/s
Thermal Shock Resistance Indexcalculated0

Values are nominal handbook figures for design screening. Certified mill or lot data ships with every FabDigit order on request.

Strength versus weight in the polymer family

Yield strength against density for every polymer grade FabDigit runs. PTMT is highlighted; hover a dot for its name, or open the interactive family chart.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scalePTMT

Working with PTMT

Is PTMT easy to machine?

Machines cleanly like acetal with sharp positive-rake tools and air cooling; glass-filled grades are abrasive — use carbide/PCD and expect edge chipping on thin sections.

Can PTMT be welded?

Ultrasonic, vibration, hot-plate and laser (with laser-transparent/absorbing pairs) welding all work well; solvent bonding is impractical, use epoxy or cyanoacrylate on abraded, flame/plasma-treated surfaces.

Can PTMT be formed, bent or molded?

Dry to <0.02 % moisture (120 °C, 3–4 h) to avoid hydrolytic MW loss; mold at 250–265 °C melt, 60–100 °C tool; fast crystallization gives short cycles but 1.4–2 % shrinkage and anisotropic warpage in GF grades.

PTMT chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
terephthalic acid / dimethyl terephthalaaromatic diacid segment of the repeat unit (wt % basis of neat polymer)≈ 6262
titanium/antimony catalyst residuepolycondensation catalyst, ppm level≈ 0.020.02
glass fiberreinforcement in GF variants; chopped E-glass with silane sizing0 – 500
flame retardant (brominated + Sb2O3 or hFR variants only0 – 200
impact modifier / stabilizer packageelastomer, antioxidant, carbodiimide hydrolysis stabilizer, HALS0 – 200.5
1,4-butanediol (tetramethylene glycol) ugives the 'PTMT' (polytetramethylene terephthalate) namebalance

What surface finishes work on PTMT?

Takes pad printing and laser marking readily; paint and metallize only after plasma/flame or primer treatment because of the low-energy, chemically resistant surface.

Equivalent designations

Standards and trade names that resolve to PTMT in FabDigit's catalog. Equivalence is nominal — check the exact specification when certification matters.

Also called
PBT

How much does PTMT cost?

PTMT is a standard-cost polymer ($$), cheaper than about 71% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

PTMT — frequently asked

What is PTMT used for?

PTMT is typically used for electrical bobbins and connectors, precision gears and bushings, automotive electrical components and consumer electronics parts. In short: legacy designation for PBT; fast-cycling engineering polyester; wide filled-grade range.

What is the yield strength of PTMT?

PTMT has a typical yield strength of 55 MPa (7.98 ksi) and a tensile strength of 55 MPa (7.98 ksi) — stronger than 62% of polymer grades. Strength varies by condition: see the 17 listed tempers.

Is PTMT easy to machine?

Reasonably — machinability is rated good (68/100, better than 71% of polymer grades). Machines cleanly like acetal with sharp positive-rake tools and air cooling; glass-filled grades are abrasive — use carbide/PCD and expect edge chipping on thin sections.

Can PTMT be welded?

Yes — weldability is rated very good (70/100). Ultrasonic, vibration, hot-plate and laser (with laser-transparent/absorbing pairs) welding all work well; solvent bonding is impractical, use epoxy or cyanoacrylate on abraded, flame/plasma-treated surfaces.

What surface finishes work on PTMT?

Takes pad printing and laser marking readily; paint and metallize only after plasma/flame or primer treatment because of the low-energy, chemically resistant surface.

Can PTMT be formed, bent or molded?

Dry to <0.02 % moisture (120 °C, 3–4 h) to avoid hydrolytic MW loss; mold at 250–265 °C melt, 60–100 °C tool; fast crystallization gives short cycles but 1.4–2 % shrinkage and anisotropic warpage in GF grades.

What is the maximum service temperature of PTMT?

PTMT is rated for continuous use to about 120°C (248 °F), and briefly to 160°C. Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

How much does PTMT cost?

PTMT is a standard-cost polymer ($$), cheaper than about 71% of the materials FabDigit quotes. Part price depends far more on geometry, tolerance and quantity than on the raw stock — upload a CAD file for a live quote.

Sources

  1. ISO 7792-1/-2 Plastics — Thermoplastic polyester (TP) moulding and extrusion materials — ISO (2012)
  2. ASTM D5927 Standard Specification for Thermoplastic Polyester (TPES) Injection and Extrusion Materials — ASTM (2020)
  3. Ultradur (PBT) product range brochure and property tables — BASF (2023)
  4. Crastin PBT thermoplastic polyester resin datasheets — DuPont / Celanese (2023)
  5. CAMPUS plastics database — PBT unfilled and GF grades — CWFG (2024)
  6. Engineered Materials Handbook Vol. 2 — Engineering Plastics — ASM International (1988)
  7. TECADUR PBT stock shapes datasheet — Ensinger (2022)

Property data is compiled from published supplier and standards handbooks and normalised for comparison; hardness values on non-Brinell scales are converted approximately for charting only. Manufacturability limits are FabDigit quote-engine defaults and may be relaxed by engineering review. Nothing on this page is a certification — request mill certs, CoC or material test reports with your order.