FabDigitFabDigit

ABS-ESD AS-PERM

Additive grade

also ABS ESD, ESD ABS

AS-PERM = permanent antistatic ABS

Pick when colour other than black is required and only antistatic (10¹⁰–10¹² Ω, no charge build-up) rather than full ESD dissipation is specified.

3D printingPremium cost $$$

Values for the AS-PERM condition

Other ABS-ESD grades and fills

ABS-ESD is listed in 5 conditions; see the grade overview at ABS-ESD.

Compare all 5 grades and fillsHide
Grade · open for datasheetBest forYield MPaTensile MPaElong. %Hardness
Carbon-nanotube ESD ABS
Use where carbon-black particle sloughing is unacceptable (wafer/optics handling) and a tighter 10⁶–10⁹ Ω window is required.3840677 Shore D
AS-PERMThis page
Permanent antistatic ABS
Pick when colour other than black is required and only antistatic (10¹⁰–10¹² Ω, no charge build-up) rather than full ESD dissipation is specified.38401575 Shore D
Flame-retardant ESD ABS
For ESD fixtures in equipment that must also meet UL 94 V-0 flammability at 1.5–3 mm.3840877 Shore D
Injection-moulding compound, carbon-black ESD ABS
Pick for volume-moulded ESD trays, carriers and housings where isotropic strength and low cost matter more than lead time.40421278 Shore D
Carbon-fibre filled conductive ABS
Choose when stiffness/low warp plus true conductive (10²–10⁵ Ω) shielding-level performance is needed rather than pure static dissipation.—552—

What is ABS-ESD AS-PERM?

ABS-ESD AS-PERM is ABS-ESD in the AS-PERM grade — pick when colour other than black is required and only antistatic (10¹⁰–10¹² Ω, no charge build-up) rather than full ESD dissipation is specified. ABS-ESD AS-PERM has a yield strength of 38 MPa (5.51 ksi) and a tensile strength of 40 MPa (5.8 ksi) — weaker than 64% of polymer grades. Elongation at break is 15% and the elastic modulus is 2.3 GPa (0.334 Msi). ABS-ESD AS-PERM has a density of 1.04 g/cm³ (0.0376 lb/in³), lighter than 71% of polymer grades. Its glass-transition temperature is 108°C (226 °F).

ABS-ESD AS-PERM properties

Typical room-temperature values for ABS-ESD AS-PERM; 26 are specific to this condition. Other listed values are ABS-ESD reference data and may not represent this condition. Bars are the position among polymer grades.

Physical4

ABS-ESD AS-PERM has a density of 1.04 g/cm³ (0.0376 lb/in³), lighter than 71% of polymer grades. Its glass-transition temperature is 108°C (226 °F).

Density1.04 g/cm³0.04 lb/in³
Glass Transition (Tg)108°C226 °F
Water Absorption (24 h)0.3%
Water Absorption (Saturation)0.8%

Mechanical12

ABS-ESD AS-PERM has a yield strength of 38 MPa (5.51 ksi) and a tensile strength of 40 MPa (5.8 ksi) — weaker than 64% of polymer grades. Elongation at break is 15% and the elastic modulus is 2.3 GPa (0.334 Msi).

Elastic (Young's) Modulus2.3 GPa0.33 Msi
Poisson's Ratio0.37
Tensile Strength (Ultimate)40 MPa5.8 ksi
Yield Strength (0.2% offset)38 MPa5.5 ksi
Elongation at Break15%
Compressive Strength50 MPa7.3 ksi
Compressive Modulus2 GPa0.29 Msi
Flexural Strength64 MPa9.3 ksi
Flexural Modulus2.3 GPa0.33 Msi
Izod Impact, Notched120 J/m2.2 ft·lbf/in
Hardness, Shore D75 Shore D
Hardness, Rockwell R103 HRR

Thermal11

ABS-ESD AS-PERM is rated for continuous service to 75°C (167 °F). It conducts heat at 0.18 W/m·K (0.104 BTU/hr·ft·°F), worse than 73% of polymer grades. Thermal expansion is 85 µm/m·K (47.2 µin/in·°F).

Thermal Conductivity0.18 W/m·K0.1 BTU/hr·ft·°F
Specific Heat Capacity1,400 J/kg·K0.33 BTU/lb·°F
Thermal Expansion (CTE, 20–100 °C)85 µm/m·K47.2 µin/in·°F
Max Service Temperature (continuous)75°C167 °F
Min Service Temperature-20°C-4 °F
Heat Deflection Temp. @ 0.45 MPa94°C201 °F
Heat Deflection Temp. @ 1.8 MPa82°C180 °F
Vicat Softening Point (B50)99°C210 °F
Flammability (UL 94)HB at 1.5–3 mm for standard ESD ABS; FR (V-0) versions available as separate compounds
Limiting Oxygen Index19%
Max Service Temperature (short-term)95°C203 °F

Electrical3

ABS-ESD AS-PERM has an electrical resistivity of 1×10⁹ Ω·m.

Electrical Resistivity1×10⁹ Ω·m3.94×10¹⁶ µΩ·in
Volume Resistivity1×10¹¹ Ω·cm
Surface Resistivity1×10¹¹ Ω

Chemical & Environmental2

UV resistance is fair.

UV / Weathering ResistanceFair45/100
Chemical Resistance SummaryGood against dilute acids/alkalis, aliphatic hydrocarbons, oils and IPA wipe-down; attacked or dissolved by ketones (acetone, MEK), esters, chlorinated solvents and aromatic hydrocarbons; prone to environmental stress cracking under load in contact with solvents.

Sustainability4

Producing a kilogram of ABS-ESD AS-PERM takes about 95 MJ of energy and emits 3.8 kg of CO₂ — less than 70% of polymer grades. Typical recycled content is 0%.

Embodied Energy (primary production)95 MJ/kg40,843 BTU/lb
Embodied Carbon (primary production)3.8 kg CO₂/kg
Embodied Water220 L/kg26.4 gal/lb
Typical Recycled Content0%

Manufacturability7

ABS-ESD AS-PERM's machinability is very good (70/100, better than 74% of polymer grades); weldability good (65/100).

MachinabilityVery good70/100
WeldabilityGood65/100
PolishabilityFair40/100
Mold Shrinkage0.55%
Melt Flow Rate8 g/10 min
Processing Melt Temperature (typ.)245°C473 °F
Mold Temperature (typ.)90°C194 °F

Values are nominal handbook figures for design screening. Confirm any required mill or lot documentation when quoting.

Working with ABS-ESD AS-PERM

Is ABS-ESD easy to machine?

Machines easily with sharp single-flute or O-flute cutters at high rpm/low feed; keep chips clear and avoid coolants containing ketones, and note that heavy sanding can locally alter surface resistivity.

Can ABS-ESD be welded?

Joins well by solvent bonding (avoid on ESD-critical surfaces), ultrasonic and hot-plate welding; conductive-filled joints may need a bridging conductive adhesive to keep the path continuous.

Can ABS-ESD be formed, bent or molded?

Dry 2–4 h at 80 °C before printing/moulding; FDM needs a 90–100 °C heated chamber and 230–265 °C nozzle to limit warping, injection at 220–250 °C melt / 50–80 °C mould with moderate shear to preserve the carbon network.

What surface finishes work on ABS-ESD?

Supplied black only; vapour smoothing or paint/primer will insulate the surface and destroy ESD function, so leave working faces as-printed or lightly bead blasted and verify surface resistance per ANSI/ESD STM11.11.

ABS-ESD chemical composition (wt %)

Limits by weight percent from the governing specification, written the way the spec states them — a single maximum for impurities, a range for alloying elements, and the base element as balance. Nominal is the typical mid-range value.

ElementSpec limit (wt %)Nominal
styrenerigid matrix phase with acrylonitrile40 – 6050
acrylonitrilechemical/heat resistance15 – 3023
polybutadiene rubberimpact-modifying elastomer phase5 – 2515
conductive carbon blackESD network; replaced by CNT or antistatic agent in other variants2 – 105
processing additives (lubricant, stabili0.5 – 31.5

ABS-ESD AS-PERM — frequently asked

What is ABS-ESD AS-PERM used for?

ABS-ESD AS-PERM is typically used for electronics jigs, PCB fixtures and component trays. In short: static-dissipative ABS.

What is the yield strength of ABS-ESD AS-PERM?

ABS-ESD AS-PERM has a typical yield strength of 38 MPa (5.51 ksi) and a tensile strength of 40 MPa (5.8 ksi) — weaker than 64% of polymer grades. Strength varies by condition: see the 5 listed tempers.

Is ABS-ESD AS-PERM easy to machine?

Yes — machinability is rated very good (70/100, better than 74% of polymer grades). Machines easily with sharp single-flute or O-flute cutters at high rpm/low feed; keep chips clear and avoid coolants containing ketones, and note that heavy sanding can locally alter surface resistivity.

Can ABS-ESD AS-PERM be welded?

Yes — weldability is rated good (65/100). Joins well by solvent bonding (avoid on ESD-critical surfaces), ultrasonic and hot-plate welding; conductive-filled joints may need a bridging conductive adhesive to keep the path continuous.

What surface finishes work on ABS-ESD AS-PERM?

Supplied black only; vapour smoothing or paint/primer will insulate the surface and destroy ESD function, so leave working faces as-printed or lightly bead blasted and verify surface resistance per ANSI/ESD STM11.11.

Can ABS-ESD AS-PERM be formed, bent or molded?

Dry 2–4 h at 80 °C before printing/moulding; FDM needs a 90–100 °C heated chamber and 230–265 °C nozzle to limit warping, injection at 220–250 °C melt / 50–80 °C mould with moderate shear to preserve the carbon network.

What is the maximum service temperature of ABS-ESD AS-PERM?

ABS-ESD AS-PERM is rated for continuous use to about 75°C (167 °F), and briefly to 95°C. Strength falls off well before that limit — check the elevated-temperature data for load-bearing parts.

Can FabDigit make parts in ABS-ESD AS-PERM?

Yes — ABS-ESD AS-PERM is available for 3D printing with instant online pricing. Upload a STEP file to get a price and a DFM check.

Sources

  1. ABS-ESD7 FDM Thermoplastic Material Data Sheet — Stratasys (2023)
  2. ANSI/ESD STM11.11 Surface Resistance Measurement of Static Dissipative Planar Materials — ESD Association (2015)
  3. ASTM D257 Standard Test Methods for DC Resistance or Conductance of Insulating Materials — ASTM (2021)
  4. Engineered Materials Handbook Vol. 2: Engineering Plastics — ASM International (1988)
  5. CAMPUS / UL Prospector ABS compound datasets — CWFG / UL (2024)