FabDigitFabDigit

Magnesium Alloy WE43B vs ZM3

Magnesium Alloy · grade comparison

Magnesium Alloy WE43B and ZM3 are both magnesium alloy grades. WE43B is the stronger of the two: yield strength 175 MPa (25.4 ksi) against 95 MPa (13.8 ksi) for ZM3, about 84% more; tensile strength follows at 255 MPa (37 ksi) vs 145 MPa (21 ksi). WE43B is the more ductile: elongation 8% versus 3% for ZM3, and WE43B is harder (85 HB vs 55 HB). ZM3 conducts heat better (100 W/m·K vs 51 W/m·K). On the shop floor, ZM3 sits in a lower cost tier (premium, $$$) than WE43B (high, $$$$).

WE43BChoose it when strength drives the design, or when the part is bent, formed or impact-loaded.

ZM3Choose it when cost is the deciding factor.

WE43B vs ZM3: properties

WE43BZM3

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Shear Modulus

16.5 GPa2.4 Msi
17 GPa2.5 Msi

Bulk Modulus

32 GPa4.6 Msi
45 GPa6.5 Msi

Poisson's Ratio

0.27
0.35

Tensile Strength (Ultimate)

255 MPa37 ksi
145 MPa21 ksi

Yield Strength (0.2% offset)

175 MPa25.4 ksi
95 MPa13.8 ksi

Elongation at Break

8%
3%

Compressive Strength

180 MPa26.1 ksi
110 MPa16 ksi

Shear Strength

155 MPa22.5 ksi
125 MPa18.1 ksi

Fatigue Strength (Endurance Limit)

95 MPa13.8 ksi
70 MPa10.2 ksi

Fracture Toughness (K_IC)

15 MPa·√m13.7 ksi·√in
12 MPa·√m10.9 ksi·√in

Charpy V-Notch Impact (RT)

4 J3 ft·lbf
3 J2.2 ft·lbf

Hardness, Brinell

85 HB
55 HB

Hardness, Vickers

90 HV
58 HV

Reduction in Area

—
3%

Same in both: Elastic (Young's) Modulus 44 GPa6.4 Msi

Physical

Density and transition temperatures.

Density

1.84 g/cm³0.07 lb/in³
1.8 g/cm³0.07 lb/in³

Same in both: Melting Point (Solidus) 545°C1,013 °F · Liquidus Temperature 640°C1,184 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

51 W/m·K29.5 BTU/hr·ft·°F
100 W/m·K57.8 BTU/hr·ft·°F

Specific Heat Capacity

966 J/kg·K0.23 BTU/lb·°F
1,000 J/kg·K0.24 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

26.7 µm/m·K14.8 µin/in·°F
26.5 µm/m·K14.7 µin/in·°F

Latent Heat of Fusion

350 J/g150 BTU/lb
360 J/g155 BTU/lb

Min Service Temperature

-196°C-321 °F
-70°C-94 °F

Same in both: Max Service Temperature (continuous) 250°C482 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

11.6 % IACS
24 % IACS

Electrical Resistivity

1.48×10⁻⁷ Ω·m5.83 µΩ·in
7×10⁻⁸ Ω·m2.76 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-1.53 V
-1.6 V

Corrosion Resistance

35 / 100
22 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

95 / 100
92 / 100

Machinability Rating (AISI 1212 = 100 %)

300%
500%

Weldability

70 / 100
65 / 100

Formability (cold)

25 / 100
8 / 100

Castability

75 / 100
88 / 100

Polishability

60 / 100
50 / 100

Same in both: Brazeability / Solderability 20 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

380 MJ/kg163,371 BTU/lb
330 MJ/kg141,875 BTU/lb

Embodied Carbon (primary production)

40 kg CO₂/kg
32 kg CO₂/kg

Typical Recycled Content

5%
25%

Same in both: Embodied Water 500 L/kg59.9 gal/lb

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

139 kN·m/kg
81 kN·m/kg

Specific Stiffness (E / density)

23.9 MN·m/kg
24.4 MN·m/kg

Modulus of Resilience

348 kJ/m³
103 kJ/m³

Thermal Diffusivity

28.7 mm²/s
55.6 mm²/s

Thermal Shock Resistance Index

11
12

Strength versus weight

Yield strength against density for every magnesium alloy grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

701001502001.41.51.61.71.8Density (g/cm³)Yield strength (MPa) — log scaleWE43BZM3

Manufacturing and finishing

CapabilityWE43BZM3
Default condition——
Relative cost$$$$ High$$$ Premium
Min. machined wall——
Best machined surface——

WE43B vs ZM3 — frequently asked

Is WE43B stronger than ZM3?

Yes. WE43B has a typical yield strength of 175 MPa (25.4 ksi) against 95 MPa (13.8 ksi) for ZM3 — about 84% more. Tensile strength is 255 MPa (37 ksi) vs 145 MPa (21 ksi).

Which is cheaper, WE43B or ZM3?

ZM3 is the lower-cost material: it sits in the premium tier ($$$) while WE43B is high ($$$$). Part price depends far more on geometry, tolerance and quantity than on raw stock — upload a CAD file for a live quote.

Which welds better, WE43B or ZM3?

WE43B. Its weldability rates very good (70/100) against good (65/100) for ZM3.

Ready to make it?

Upload a CAD file and FabDigit prices the part in WE43B and ZM3 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.