FabDigitFabDigit

Steel 5130 Annealed vs 5130-CD

Steel · 5130 temper comparison

5130 Annealed and 5130-CD are two conditions of the same steel grade, 5130: Annealed versus CD (cold drawn). The chemistry is identical, so every difference below comes from the condition. 5130-CD is the stronger of the two: yield strength 580 MPa (84.1 ksi) against 380 MPa (55.1 ksi) for 5130 Annealed, about 53% more; tensile strength follows at 680 MPa (98.6 ksi) vs 590 MPa (85.6 ksi). In exchange, 5130 Annealed is the more ductile: elongation 26% versus 12% for 5130-CD, and 5130-CD is harder (200 HB vs 170 HB). On the shop floor, 5130 Annealed welds better (50 vs 40 out of 100).

5130 AnnealedChoose it when the part is bent, formed or impact-loaded, or when it will be welded.

5130-CDChoose it when strength drives the design.

5130 Annealed vs 5130-CD: properties

5130 Annealed5130-CD

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

590 MPa85.6 ksi
680 MPa98.6 ksi

Yield Strength (0.2% offset)

380 MPa55.1 ksi
580 MPa84.1 ksi

Elongation at Break

26%
12%

Reduction in Area

62%
42%

Compressive Strength

380 MPa55.1 ksi
415 MPa60.2 ksi

Shear Strength

390 MPa56.6 ksi
410 MPa59.5 ksi

Fatigue Strength (Endurance Limit)

275 MPa39.9 ksi
300 MPa43.5 ksi

Fracture Toughness (K_IC)

110 MPa·√m100 ksi·√in
100 MPa·√m91 ksi·√in

Charpy V-Notch Impact (RT)

50 J36.9 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

170 HB
200 HB

Hardness, Rockwell B

86 HRB
93 HRB

Hardness, Vickers

179 HV
210 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

46 W/m·K26.6 BTU/hr·ft·°F
45 W/m·K26 BTU/hr·ft·°F

Specific Heat Capacity

477 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Same in both: Thermal Expansion (CTE, 20–100 °C) 12.2 µm/m·K6.8 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Max Service Temperature (continuous) 400°C752 °F · Min Service Temperature -30°C-22 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

8.5 % IACS
8 % IACS

Electrical Resistivity

2.1×10⁻⁷ Ω·m8.27 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

62 / 100
60 / 100

Weldability

50 / 100
40 / 100

Formability (cold)

60 / 100
35 / 100

Same in both: Machinability Rating (AISI 1212 = 100 %) 70% · Brazeability / Solderability 60 / 100 · Polishability 65 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

25 MJ/kg10,748 BTU/lb
34 MJ/kg14,617 BTU/lb

Embodied Carbon (primary production)

1.9 kg CO₂/kg
2.3 kg CO₂/kg

Same in both: Embodied Water 40 L/kg4.8 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale5130

5130 Annealed vs 5130-CD — frequently asked

Is 5130-CD stronger than 5130 Annealed?

Yes. 5130-CD has a typical yield strength of 580 MPa (84.1 ksi) against 380 MPa (55.1 ksi) for 5130 Annealed — about 53% more. Tensile strength is 680 MPa (98.6 ksi) vs 590 MPa (85.6 ksi).

Which condition does FabDigit quote by default, Annealed or CD?

HR is the default 5130 condition in the FabDigit quote flow (neither Annealed nor CD). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which welds better, 5130 Annealed or 5130-CD?

5130 Annealed. Its weldability rates fair (50/100) against fair (40/100) for 5130-CD.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 5130 Annealed and 5130-CD side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.