Ti Grade 4 Annealed and Ti Grade 4-SR are two conditions of the same titanium grade, Ti Grade 4: Annealed versus SR (stress relieved). The chemistry is identical, so every difference below comes from the condition. Both yield at about 520 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (Annealed versus stress relieved). Ti Grade 4 Annealed is the more ductile: elongation 20% versus 18% for Ti Grade 4-SR.

Ti Grade 4 AnnealedChoose it when the part is bent, formed or impact-loaded.

Ti Grade 4 Annealed vs Ti Grade 4-SR: properties

Ti Grade 4 AnnealedTi Grade 4-SR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

620 MPa89.9 ksi
640 MPa92.8 ksi

Yield Strength (0.2% offset)

520 MPa75.4 ksi
545 MPa79 ksi

Elongation at Break

20%
18%

Reduction in Area

40%
38%

Compressive Strength

550 MPa79.8 ksi
575 MPa83.4 ksi

Shear Strength

400 MPa58 ksi
415 MPa60.2 ksi

Fatigue Strength (Endurance Limit)

320 MPa46.4 ksi
340 MPa49.3 ksi

Fracture Toughness (K_IC)

70 MPa·√m63.7 ksi·√in
68 MPa·√m61.9 ksi·√in

Charpy V-Notch Impact (RT)

20 J14.8 ft·lbf
18 J13.3 ft·lbf

Hardness, Brinell

250 HB
260 HB

Hardness, Rockwell C

24 HRC
25 HRC

Hardness, Vickers

260 HV
270 HV

Same in both: Elastic (Young's) Modulus 105 GPa15.2 Msi · Shear Modulus 45 GPa6.5 Msi · Bulk Modulus 110 GPa16 Msi · Poisson's Ratio 0.34

Physical

Density and transition temperatures.

Same in both: Density 4.51 g/cm³0.16 lb/in³ · Melting Point (Solidus) 1,660°C3,020 °F · Liquidus Temperature 1,670°C3,038 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 17 W/m·K9.8 BTU/hr·ft·°F · Specific Heat Capacity 540 J/kg·K0.13 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 8.6 µm/m·K4.8 µin/in·°F · Latent Heat of Fusion 295 J/g127 BTU/lb · Max Service Temperature (continuous) 300°C572 °F · Min Service Temperature -100°C-148 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 3.1 % IACS · Electrical Resistivity 5.6×10⁻⁷ Ω·m22 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.1 V · Corrosion Resistance 92 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

30 / 100
28 / 100

Machinability Rating (AISI 1212 = 100 %)

28%
26%

Formability (cold)

40 / 100
35 / 100

Same in both: Weldability 85 / 100 · Castability 35 / 100 · Brazeability / Solderability 40 / 100 · Polishability 75 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 650 MJ/kg279,450 BTU/lb · Embodied Carbon (primary production) 45 kg CO₂/kg · Embodied Water 900 L/kg108 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every titanium grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

3005007001,0004.555.5Density (g/cm³)Yield strength (MPa) — log scaleTi Grade 4

Ti Grade 4 Annealed vs Ti Grade 4-SR — frequently asked

What is the difference between Ti Grade 4 Annealed and Ti Grade 4-SR?

Ti Grade 4 Annealed and Ti Grade 4-SR are two conditions of the same titanium grade, Ti Grade 4: Annealed versus SR (stress relieved). The chemistry is identical, so every difference below comes from the condition. Both yield at about 520 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (Annealed versus stress relieved).

Which condition does FabDigit quote by default, Annealed or SR?

Annealed is the default Ti Grade 4 condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose Ti Grade 4 Annealed over Ti Grade 4-SR?

Pick Ti Grade 4 Annealed when the part is bent, formed or impact-loaded.