Titanium Ti Grade 25 Annealed vs Ti Grade 25 Beta Annealed

Titanium · Ti Grade 25 temper comparison

Ti Grade 25 Annealed and Ti Grade 25 Beta Annealed are two conditions of the same titanium grade, Ti Grade 25: Annealed versus Beta Annealed (above beta transus anneal, slow cooled). The chemistry is identical, so every difference below comes from the condition. Both yield at about 880 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (Annealed versus above beta transus anneal, slow cooled). Ti Grade 25 Annealed is the more ductile: elongation 14% versus 10% for Ti Grade 25 Beta Annealed.

Ti Grade 25 AnnealedChoose it when the part is bent, formed or impact-loaded.

Ti Grade 25 Annealed vs Ti Grade 25 Beta Annealed: properties

Ti Grade 25 AnnealedTi Grade 25 Beta Annealed

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

950 MPa138 ksi
940 MPa136 ksi

Yield Strength (0.2% offset)

880 MPa128 ksi
860 MPa125 ksi

Elongation at Break

14%
10%

Reduction in Area

36%
20%

Compressive Strength

970 MPa141 ksi
950 MPa138 ksi

Shear Strength

550 MPa79.8 ksi
540 MPa78.3 ksi

Fatigue Strength (Endurance Limit)

500 MPa72.5 ksi
430 MPa62.4 ksi

Fracture Toughness (K_IC)

75 MPa·√m68.3 ksi·√in
90 MPa·√m81.9 ksi·√in

Charpy V-Notch Impact (RT)

17 J12.5 ft·lbf
22 J16.2 ft·lbf

Hardness, Brinell

330 HB
319 HB

Hardness, Rockwell C

35 HRC
34 HRC

Hardness, Vickers

345 HV
335 HV

Same in both: Elastic (Young's) Modulus 113 GPa16.4 Msi · Shear Modulus 44 GPa6.4 Msi · Bulk Modulus 110 GPa16 Msi · Poisson's Ratio 0.34

Physical

Density and transition temperatures.

Same in both: Density 4.43 g/cm³0.16 lb/in³ · Melting Point (Solidus) 1,604°C2,919 °F · Liquidus Temperature 1,660°C3,020 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

6.7 W/m·K3.9 BTU/hr·ft·°F
7 W/m·K4 BTU/hr·ft·°F

Same in both: Specific Heat Capacity 526 J/kg·K0.13 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 8.7 µm/m·K4.8 µin/in·°F · Latent Heat of Fusion 365 J/g157 BTU/lb · Max Service Temperature (continuous) 400°C752 °F · Min Service Temperature -196°C-321 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 1 % IACS · Electrical Resistivity 1.7×10⁻⁶ Ω·m66.9 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.08 V · Corrosion Resistance 95 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Formability (cold)

25 / 100
18 / 100

Same in both: Machinability 20 / 100 · Machinability Rating (AISI 1212 = 100 %) 22% · Weldability 65 / 100 · Castability 35 / 100 · Brazeability / Solderability 35 / 100 · Polishability 75 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 640 MJ/kg275,151 BTU/lb · Embodied Carbon (primary production) 35 kg CO₂/kg · Embodied Water 1,200 L/kg144 gal/lb · Typical Recycled Content 25%

Strength versus weight

Yield strength against density for every titanium grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

3005007001,0004.555.5Density (g/cm³)Yield strength (MPa) — log scaleTi Grade 25

Ti Grade 25 Annealed vs Ti Grade 25 Beta Annealed — frequently asked

What is the difference between Ti Grade 25 Annealed and Ti Grade 25 Beta Annealed?

Ti Grade 25 Annealed and Ti Grade 25 Beta Annealed are two conditions of the same titanium grade, Ti Grade 25: Annealed versus Beta Annealed (above beta transus anneal, slow cooled). The chemistry is identical, so every difference below comes from the condition. Both yield at about 880 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (Annealed versus above beta transus anneal, slow cooled).

Which condition does FabDigit quote by default, Annealed or Beta Annealed?

Annealed is the default Ti Grade 25 condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose Ti Grade 25 Annealed over Ti Grade 25 Beta Annealed?

Pick Ti Grade 25 Annealed when the part is bent, formed or impact-loaded.

Ready to make it?

Upload a CAD file and FabDigit prices the part in Ti Grade 25 Annealed and Ti Grade 25 Beta Annealed side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.