FabDigitFabDigit

Steel Q460-N vs Q460-NH

Steel · Q460 temper comparison

Q460-N and Q460-NH are two conditions of the same steel grade, Q460: N (normalized) versus NH (weathering (atmospheric corrosion resistant) steel Q460NH, GB/T 4171). The chemistry is identical, so every difference below comes from the condition. Both yield at about 505 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (normalized versus weathering (atmospheric corrosion resistant) steel Q460NH, GB/T 4171). For most parts the choice follows the drawing's specified condition; ask for the one your standard calls out.

Q460-N vs Q460-NH: properties

Q460-NQ460-NH

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

630 MPa91.4 ksi
620 MPa89.9 ksi

Yield Strength (0.2% offset)

505 MPa73.2 ksi
500 MPa72.5 ksi

Elongation at Break

22%
20%

Reduction in Area

56%
50%

Compressive Strength

505 MPa73.2 ksi
500 MPa72.5 ksi

Shear Strength

385 MPa55.8 ksi
380 MPa55.1 ksi

Fatigue Strength (Endurance Limit)

285 MPa41.3 ksi
275 MPa39.9 ksi

Fracture Toughness (K_IC)

115 MPa·√m105 ksi·√in
100 MPa·√m91 ksi·√in

Charpy V-Notch Impact (RT)

90 J66.4 ft·lbf
80 J59 ft·lbf

Hardness, Brinell

185 HB
190 HB

Hardness, Rockwell B

90 HRB
91 HRB

Hardness, Vickers

195 HV
200 HV

Same in both: Elastic (Young's) Modulus 206 GPa29.9 Msi · Shear Modulus 79 GPa11.5 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.3

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

45 W/m·K26 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Max Service Temperature (continuous)

380°C716 °F
350°C662 °F

Min Service Temperature

-40°C-40 °F
0°C32 °F

Same in both: Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Latent Heat of Fusion 260 J/g112 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

8.2 % IACS
7.6 % IACS

Electrical Resistivity

2.1×10⁻⁷ Ω·m8.27 µΩ·in
2.3×10⁻⁷ Ω·m9.06 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

12 / 100
28 / 100

Same in both: Galvanic Potential (seawater, vs SCE) -0.62 V

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

54 / 100
50 / 100

Machinability Rating (AISI 1212 = 100 %)

57%
52%

Weldability

74 / 100
68 / 100

Formability (cold)

60 / 100
52 / 100

Same in both: Castability 30 / 100 · Brazeability / Solderability 55 / 100 · Polishability 45 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 26 MJ/kg11,178 BTU/lb · Embodied Carbon (primary production) 2.1 kg CO₂/kg · Embodied Water 45 L/kg5.4 gal/lb · Typical Recycled Content 25%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleQ460

Q460-N vs Q460-NH — frequently asked

What is the difference between Q460-N and Q460-NH?

Q460-N and Q460-NH are two conditions of the same steel grade, Q460: N (normalized) versus NH (weathering (atmospheric corrosion resistant) steel Q460NH, GB/T 4171). The chemistry is identical, so every difference below comes from the condition. Both yield at about 505 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (normalized versus weathering (atmospheric corrosion resistant) steel Q460NH, GB/T 4171).

Which condition does FabDigit quote by default, N or NH?

HR is the default Q460 condition in the FabDigit quote flow (neither N nor NH). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which welds better, Q460-N or Q460-NH?

Q460-N. Its weldability rates very good (74/100) against good (68/100) for Q460-NH.