EN36-CD and EN36-HR are two conditions of the same steel grade, EN36: CD (cold drawn) versus HR (hot rolled). The chemistry is identical, so every difference below comes from the condition. EN36-CD is the stronger of the two: yield strength 620 MPa (89.9 ksi) against 450 MPa (65.3 ksi) for EN36-HR, about 38% more; tensile strength follows at 810 MPa (117 ksi) vs 700 MPa (102 ksi). In exchange, EN36-HR is the more ductile: elongation 18% versus 11% for EN36-CD, and EN36-CD is harder (235 HB vs 200 HB).

EN36-CDChoose it when strength drives the design.

EN36-HRChoose it when the part is bent, formed or impact-loaded.

EN36-CD vs EN36-HR: properties

EN36-CDEN36-HR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

810 MPa117 ksi
700 MPa102 ksi

Yield Strength (0.2% offset)

620 MPa89.9 ksi
450 MPa65.3 ksi

Elongation at Break

11%
18%

Reduction in Area

42%
50%

Compressive Strength

635 MPa92.1 ksi
460 MPa66.7 ksi

Shear Strength

490 MPa71.1 ksi
425 MPa61.6 ksi

Fatigue Strength (Endurance Limit)

370 MPa53.7 ksi
330 MPa47.9 ksi

Fracture Toughness (K_IC)

90 MPa·√m81.9 ksi·√in
100 MPa·√m91 ksi·√in

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
55 J40.6 ft·lbf

Hardness, Brinell

235 HB
200 HB

Hardness, Rockwell B

99 HRB
93 HRB

Hardness, Vickers

248 HV
210 HV

Same in both: Elastic (Young's) Modulus 207 GPa30 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 165 GPa23.9 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,425°C2,597 °F · Liquidus Temperature 1,490°C2,714 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 36 W/m·K20.8 BTU/hr·ft·°F · Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Latent Heat of Fusion 270 J/g116 BTU/lb · Max Service Temperature (continuous) 250°C482 °F · Min Service Temperature -60°C-76 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 6.5 % IACS · Electrical Resistivity 2.7×10⁻⁷ Ω·m10.6 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.6 V · Corrosion Resistance 14 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

52 / 100
45 / 100

Machinability Rating (AISI 1212 = 100 %)

58%
50%

Weldability

28 / 100
30 / 100

Formability (cold)

30 / 100
45 / 100

Same in both: Brazeability / Solderability 55 / 100 · Polishability 60 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 32 MJ/kg13,758 BTU/lb · Embodied Carbon (primary production) 2.4 kg CO₂/kg · Embodied Water 65 L/kg7.8 gal/lb · Typical Recycled Content 25%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleEN36

EN36-CD vs EN36-HR — frequently asked

Is EN36-CD stronger than EN36-HR?

Yes. EN36-CD has a typical yield strength of 620 MPa (89.9 ksi) against 450 MPa (65.3 ksi) for EN36-HR — about 38% more. Tensile strength is 810 MPa (117 ksi) vs 700 MPa (102 ksi).

Which condition does FabDigit quote by default, CD or HR?

HR is the default EN36 condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, EN36-CD or EN36-HR?

EN36-CD, by a small margin. Both rate fair for machinability — 52/100 against 45/100 for EN36-HR.

Ready to make it?

Upload a CAD file and FabDigit prices the part in EN36-CD and EN36-HR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.