1025-CD and 1025-QT are two conditions of the same steel grade, 1025: CD (cold drawn) versus QT (quenched and tempered). The chemistry is identical, so every difference below comes from the condition. 1025-QT is the stronger of the two: tensile strength 550 MPa (79.8 ksi) against 440 MPa (63.8 ksi) for 1025-CD, about 25% more. 1025-QT is the more ductile: elongation 20% versus 15% for 1025-CD, and 1025-QT is harder (170 HB vs 126 HB).

1025-QTChoose it when strength drives the design, or when the part is bent, formed or impact-loaded.

1025-CD vs 1025-QT: properties

1025-CD1025-QT

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

440 MPa63.8 ksi
550 MPa79.8 ksi

Yield Strength (0.2% offset)

370 MPa53.7 ksi
380 MPa55.1 ksi

Elongation at Break

15%
20%

Reduction in Area

40%
55%

Compressive Strength

220 MPa31.9 ksi
380 MPa55.1 ksi

Shear Strength

275 MPa39.9 ksi
370 MPa53.7 ksi

Fatigue Strength (Endurance Limit)

220 MPa31.9 ksi
260 MPa37.7 ksi

Fracture Toughness (K_IC)

90 MPa·√m81.9 ksi·√in
80 MPa·√m72.8 ksi·√in

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
70 J51.6 ft·lbf

Hardness, Brinell

126 HB
170 HB

Hardness, Rockwell B

71 HRB
88 HRB

Hardness, Vickers

122 HV
180 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.87 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,425°C2,597 °F · Liquidus Temperature 1,515°C2,759 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

51.9 W/m·K30 BTU/hr·ft·°F
49 W/m·K28.3 BTU/hr·ft·°F

Same in both: Specific Heat Capacity 486 J/kg·K0.12 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Max Service Temperature (continuous) 400°C752 °F · Min Service Temperature -20°C-4 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

10.5 % IACS
10 % IACS

Electrical Resistivity

1.65×10⁻⁷ Ω·m6.5 µΩ·in
1.72×10⁻⁷ Ω·m6.77 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

60 / 100
52 / 100

Machinability Rating (AISI 1212 = 100 %)

70%
60%

Weldability

85 / 100
80 / 100

Formability (cold)

50 / 100
45 / 100

Same in both: Brazeability / Solderability 75 / 100 · Polishability 50 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 2 kg CO₂/kg · Embodied Water 45 L/kg5.4 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale1025

1025-CD vs 1025-QT — frequently asked

Is 1025-QT stronger than 1025-CD?

Yes. 1025-QT has a typical tensile strength of 550 MPa (79.8 ksi) against 440 MPa (63.8 ksi) for 1025-CD — about 25% more.

Which condition does FabDigit quote by default, CD or QT?

HR is the default 1025 condition in the FabDigit quote flow (neither CD nor QT). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 1025-CD or 1025-QT?

1025-CD. Its machinability rates good (60/100) against fair (52/100) for 1025-QT; for welding the order is 1025-CD first (excellent, 85/100) then 1025-QT (very good, 80/100).

Ready to make it?

Upload a CAD file and FabDigit prices the part in 1025-CD and 1025-QT side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.