FabDigitFabDigit

Copper Alloy CC480K-GC vs CC480K-GS

Copper Alloy · CC480K temper comparison

CC480K-GC and CC480K-GS are two conditions of the same copper alloy grade, CC480K: GC (continuous cast bar / tube) versus GS (sand cast). The chemistry is identical, so every difference below comes from the condition. CC480K-GC is the stronger of the two: yield strength 190 MPa (27.6 ksi) against 150 MPa (21.8 ksi) for CC480K-GS, about 27% more; tensile strength follows at 330 MPa (47.9 ksi) vs 290 MPa (42.1 ksi). In exchange, CC480K-GS is the more ductile: elongation 10% versus 8% for CC480K-GC, and CC480K-GC is harder (95 HB vs 85 HB).

CC480K-GCChoose it when strength drives the design.

CC480K-GSChoose it when the part is bent, formed or impact-loaded.

CC480K-GC vs CC480K-GS: properties

CC480K-GCCC480K-GS

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

103 GPa14.9 Msi
100 GPa14.5 Msi

Tensile Strength (Ultimate)

330 MPa47.9 ksi
290 MPa42.1 ksi

Yield Strength (0.2% offset)

190 MPa27.6 ksi
150 MPa21.8 ksi

Elongation at Break

8%
10%

Compressive Strength

420 MPa60.9 ksi
380 MPa55.1 ksi

Shear Strength

215 MPa31.2 ksi
200 MPa29 ksi

Fatigue Strength (Endurance Limit)

125 MPa18.1 ksi
105 MPa15.2 ksi

Charpy V-Notch Impact (RT)

10 J7.4 ft·lbf
9 J6.6 ft·lbf

Hardness, Brinell

95 HB
85 HB

Hardness, Rockwell B

55 HRB
45 HRB

Same in both: Shear Modulus 40 GPa5.8 Msi · Bulk Modulus 110 GPa16 Msi · Poisson's Ratio 0.34

Physical

Density and transition temperatures.

Same in both: Density 8.8 g/cm³0.32 lb/in³ · Melting Point (Solidus) 830°C1,526 °F · Liquidus Temperature 1,000°C1,832 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

60 W/m·K34.7 BTU/hr·ft·°F
58 W/m·K33.5 BTU/hr·ft·°F

Same in both: Specific Heat Capacity 377 J/kg·K0.09 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 18.5 µm/m·K10.3 µin/in·°F · Latent Heat of Fusion 170 J/g73.1 BTU/lb · Max Service Temperature (continuous) 250°C482 °F · Min Service Temperature -200°C-328 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

12 % IACS
11.5 % IACS

Electrical Resistivity

1.44×10⁻⁷ Ω·m5.67 µΩ·in
1.5×10⁻⁷ Ω·m5.91 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

70 / 100
68 / 100

Same in both: Galvanic Potential (seawater, vs SCE) -0.26 V

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
40 / 100

Same in both: Machinability Rating (AISI 1212 = 100 %) 30% · Weldability 25 / 100 · Formability (cold) 5 / 100 · Castability 80 / 100 · Brazeability / Solderability 82 / 100 · Polishability 70 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 60 MJ/kg25,795 BTU/lb · Embodied Carbon (primary production) 4.2 kg CO₂/kg · Embodied Water 320 L/kg38.3 gal/lb · Typical Recycled Content 60%

Strength versus weight

Yield strength against density for every copper alloy grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

501002005001,0007.588.599.5Density (g/cm³)Yield strength (MPa) — log scaleCC480K

CC480K-GC vs CC480K-GS — frequently asked

Is CC480K-GC stronger than CC480K-GS?

Yes. CC480K-GC has a typical yield strength of 190 MPa (27.6 ksi) against 150 MPa (21.8 ksi) for CC480K-GS — about 27% more. Tensile strength is 330 MPa (47.9 ksi) vs 290 MPa (42.1 ksi).

Which condition does FabDigit quote by default, GC or GS?

GC is the default CC480K condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, CC480K-GC or CC480K-GS?

CC480K-GC, by a small margin. Both rate fair for machinability — 45/100 against 40/100 for CC480K-GS.

Ready to make it?

Upload a CAD file and FabDigit prices the part in CC480K-GC and CC480K-GS side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.