FabDigit

SUP9 vs 5160 and 2 more: properties

SUP9516055Cr360Si2MnA

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

206 GPa29.9 Msi
205 GPa29.7 Msi
206 GPa29.9 Msi
206 GPa29.9 Msi

Shear Modulus

79 GPa11.5 Msi
80 GPa11.6 Msi
79.5 GPa11.5 Msi
79 GPa11.5 Msi

Tensile Strength (Ultimate)

760 MPa110 ksi
725 MPa105 ksi
800 MPa116 ksi
900 MPa131 ksi

Yield Strength (0.2% offset)

440 MPa63.8 ksi
275 MPa39.9 ksi
480 MPa69.6 ksi
550 MPa79.8 ksi

Elongation at Break

22%
17%
16%
14%

Reduction in Area

50%
31%
40%
40%

Shear Strength

480 MPa69.6 ksi
450 MPa65.3 ksi
500 MPa72.5 ksi
560 MPa81.2 ksi

Fatigue Strength (Endurance Limit)

350 MPa50.8 ksi
330 MPa47.9 ksi
360 MPa52.2 ksi
420 MPa60.9 ksi

Charpy V-Notch Impact (RT)

30 J22.1 ft·lbf
25 J18.4 ft·lbf
30 J22.1 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

217 HB
197 HB
225 HB
260 HB

Hardness, Rockwell B

95 HRB
92 HRB
98 HRB
100 HRB

Hardness, Vickers

228 HV
236 HV
270 HV

Compressive Strength

480 MPa69.6 ksi

Fracture Toughness (K_IC)

85 MPa·√m77.4 ksi·√in

Hardness, Rockwell C

20 HRC

Same in both: Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,420°C2,588 °F
1,425°C2,597 °F
1,420°C2,588 °F
1,450°C2,642 °F

Liquidus Temperature

1,490°C2,714 °F
1,490°C2,714 °F
1,490°C2,714 °F
1,495°C2,723 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

46 W/m·K26.6 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
37 W/m·K21.4 BTU/hr·ft·°F

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
490 J/kg·K0.12 BTU/lb·°F
465 J/kg·K0.11 BTU/lb·°F
480 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.5 µm/m·K6.9 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Max Service Temperature (continuous)

250°C482 °F
250°C482 °F
400°C752 °F
200°C392 °F

Same in both: Latent Heat of Fusion 250 J/g107 BTU/lb · Min Service Temperature -40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.8 % IACS
7.8 % IACS
7.8 % IACS
6 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.9×10⁻⁷ Ω·m11.4 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.62 V
-0.61 V

Corrosion Resistance

11 / 100
10 / 100
10 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
55 / 100
50 / 100
45 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
56%
55%
55%

Weldability

30 / 100
25 / 100
25 / 100
25 / 100

Brazeability / Solderability

50 / 100
55 / 100
40 / 100
45 / 100

Polishability

60 / 100
70 / 100
60 / 100
60 / 100

Castability

40 / 100

Same in both: Formability (cold) 45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

26 MJ/kg11,178 BTU/lb
30 MJ/kg12,898 BTU/lb
26 MJ/kg11,178 BTU/lb
26 MJ/kg11,178 BTU/lb

Embodied Carbon (primary production)

2 kg CO₂/kg
2.2 kg CO₂/kg
2 kg CO₂/kg
2 kg CO₂/kg

Embodied Water

55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb

Typical Recycled Content

30%
35%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

97 kN·m/kg
92 kN·m/kg
102 kN·m/kg
115 kN·m/kg

Specific Stiffness (E / density)

26.2 MN·m/kg
26.1 MN·m/kg
26.2 MN·m/kg
26.2 MN·m/kg

Modulus of Resilience

470 kJ/m³
184 kJ/m³
559 kJ/m³
734 kJ/m³

Thermal Diffusivity

12.5 mm²/s
12 mm²/s
12.1 mm²/s
9.8 mm²/s

Thermal Shock Resistance Index

14
13
14
14

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale516055Cr360Si2MnASUP9

Manufacturing and finishing

CapabilitySUP9516055Cr360Si2MnA
Default conditionAnnealedAnnealedAnnealedAnnealed
Relative cost$$ Standard$$$ Premium$$ Standard$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SUP9 and 5160 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.