Shear Modulus

80 GPa11.6 Msi
80 GPa11.6 Msi
81 GPa11.7 Msi
81 GPa11.7 Msi

Bulk Modulus

165 GPa23.9 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi
165 GPa23.9 Msi

Poisson's Ratio

0.29
0.3
0.3
0.29

Tensile Strength (Ultimate)

1,250 MPa181 ksi
1,600 MPa232 ksi
2,000 MPa290 ksi
1,250 MPa181 ksi

Yield Strength (0.2% offset)

1,050 MPa152 ksi
1,300 MPa189 ksi
1,650 MPa239 ksi
1,000 MPa145 ksi

Elongation at Break

12%
8%
7%
10%

Reduction in Area

40%
30%
40%

Compressive Strength

1,100 MPa160 ksi
1,300 MPa189 ksi
1,700 MPa247 ksi
1,000 MPa145 ksi

Shear Strength

750 MPa109 ksi
960 MPa139 ksi
1,200 MPa174 ksi
750 MPa109 ksi

Fatigue Strength (Endurance Limit)

550 MPa79.8 ksi
650 MPa94.3 ksi
750 MPa109 ksi
550 MPa79.8 ksi

Fracture Toughness (K_IC)

70 MPa·√m63.7 ksi·√in
60 MPa·√m54.6 ksi·√in
45 MPa·√m41 ksi·√in
80 MPa·√m72.8 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
40 J29.5 ft·lbf
20 J14.8 ft·lbf
55 J40.6 ft·lbf

Hardness, Brinell

400 HB
500 HB
600 HB
400 HB

Hardness, Rockwell C

42 HRC
50 HRC
57 HRC
43 HRC

Hardness, Vickers

420 HV
530 HV
635 HV
420 HV

Same in both: Elastic (Young's) Modulus 210 GPa30.5 Msi

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,425°C2,597 °F
1,420°C2,588 °F
1,450°C2,642 °F
1,420°C2,588 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

40 W/m·K23.1 BTU/hr·ft·°F
30 W/m·K17.3 BTU/hr·ft·°F
30 W/m·K17.3 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Same in both: Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Max Service Temperature (continuous) 250°C482 °F · Min Service Temperature -40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

8 % IACS
6 % IACS
7 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
3×10⁻⁷ Ω·m11.8 µΩ·in
2.7×10⁻⁷ Ω·m10.6 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.62 V
-0.62 V
-0.6 V
-0.61 V

Corrosion Resistance

12 / 100
12 / 100
15 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

25 / 100
22 / 100
8 / 100
25 / 100

Machinability Rating (AISI 1212 = 100 %)

25%
18%
7%
25%

Weldability

55 / 100
55 / 100
30 / 100
60 / 100

Formability (cold)

30 / 100
25 / 100
12 / 100
40 / 100

Brazeability / Solderability

30 / 100
25 / 100

Polishability

55 / 100
60 / 100
55 / 100
45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

30 MJ/kg12,898 BTU/lb
30 MJ/kg12,898 BTU/lb
30 MJ/kg12,898 BTU/lb
31 MJ/kg13,328 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.2 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
40 L/kg4.8 gal/lb
50 L/kg6 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

20%
25%
25%
25%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

159 kN·m/kg
204 kN·m/kg
255 kN·m/kg
159 kN·m/kg

Modulus of Resilience

2,625 kJ/m³
4,024 kJ/m³
6,482 kJ/m³
2,381 kJ/m³

Thermal Diffusivity

10.8 mm²/s
8.1 mm²/s
8.1 mm²/s
11.4 mm²/s

Thermal Shock Resistance Index

20
19
24
21

Same in both: Specific Stiffness (E / density) 26.8 MN·m/kg

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleHardox 500NM400Hardox 600XAR 400

Manufacturing and finishing

CapabilityNM400Hardox 500Hardox 600XAR 400
CNC machiningYesYes
Sheet metalYesYes
Default conditionQ&TQ&T
Relative cost$$ Standard$$ Standard$$ Standard$ Budget
Min. machined wall0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µm
AlCrNYesYes
AlTiNYesYes
Black OxideYesYes
CVD Al2O3YesYes
CVD TiCNYesYes
CVD TiNYesYes
CerakoteYesYes
Chrome PlatingYesYes
CrNYesYes
DLCYesYes
E-CoatingYesYes
HVOF CoatingYesYes
Hot-Dip GalvanizingYesYes
MoS2YesYes
Multilayer CVDYesYes
Nickel PlatingYesYes
PTFE CoatingYesYes
PaintingYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in NM400 and Hardox 500 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.