FabDigit

NAK80 vs P20 and 2 more: properties

NAK80P201.2344718H

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
205 GPa29.7 Msi
210 GPa30.5 Msi
205 GPa29.7 Msi

Shear Modulus

80 GPa11.6 Msi
80 GPa11.6 Msi
81 GPa11.7 Msi
80 GPa11.6 Msi

Bulk Modulus

162 GPa23.5 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi

Poisson's Ratio

0.29
0.29
0.3
0.29

Tensile Strength (Ultimate)

900 MPa131 ksi
700 MPa102 ksi
800 MPa116 ksi
1,080 MPa157 ksi

Yield Strength (0.2% offset)

700 MPa102 ksi
440 MPa63.8 ksi
500 MPa72.5 ksi
900 MPa131 ksi

Elongation at Break

18%
20%
20%
13%

Reduction in Area

45%
55%
45%
45%

Compressive Strength

1,200 MPa174 ksi
900 MPa131 ksi
520 MPa75.4 ksi

Shear Strength

780 MPa113 ksi
620 MPa89.9 ksi
480 MPa69.6 ksi
650 MPa94.3 ksi

Fatigue Strength (Endurance Limit)

600 MPa87 ksi
460 MPa66.7 ksi
360 MPa52.2 ksi
500 MPa72.5 ksi

Fracture Toughness (K_IC)

60 MPa·√m54.6 ksi·√in
65 MPa·√m59.2 ksi·√in
70 MPa·√m63.7 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
45 J33.2 ft·lbf
30 J22.1 ft·lbf
22 J16.2 ft·lbf

Hardness, Brinell

270 HB
200 HB
215 HB
300 HB

Hardness, Rockwell C

28 HRC
31 HRC
32 HRC

Hardness, Vickers

400 HV
315 HV
225 HV
320 HV

Hardness, Rockwell B

93 HRB
96 HRB

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,420°C2,588 °F
1,420°C2,588 °F
1,427°C2,601 °F
1,420°C2,588 °F

Liquidus Temperature

1,480°C2,696 °F
1,482°C2,700 °F
1,480°C2,696 °F

Same in both: Density 7.8 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

30 W/m·K17.3 BTU/hr·ft·°F
32 W/m·K18.5 BTU/hr·ft·°F
24.5 W/m·K14.2 BTU/hr·ft·°F
33 W/m·K19.1 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

12.5 µm/m·K6.9 µin/in·°F
12.4 µm/m·K6.9 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F
12.5 µm/m·K6.9 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
450°C842 °F
400°C752 °F
450°C842 °F

Min Service Temperature

-40°C-40 °F
-20°C-4 °F
-40°C-40 °F
-20°C-4 °F

Same in both: Specific Heat Capacity 460 J/kg·K0.11 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Conductivity

5.7 % IACS
3.3 % IACS

Electrical Resistivity

3×10⁻⁷ Ω·m11.8 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
5.2×10⁻⁷ Ω·m20.5 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

20 / 100
15 / 100
20 / 100
15 / 100

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.58 V

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

70 / 100
65 / 100
45 / 100
48 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
75%
55%
60%

Weldability

50 / 100
50 / 100
35 / 100
40 / 100

Formability (cold)

30 / 100
30 / 100
20 / 100
10 / 100

Brazeability / Solderability

40 / 100
40 / 100
30 / 100
40 / 100

Polishability

75 / 100
55 / 100
70 / 100
80 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

36 MJ/kg15,477 BTU/lb
32 MJ/kg13,758 BTU/lb
36 MJ/kg15,477 BTU/lb
34 MJ/kg14,617 BTU/lb

Embodied Carbon (primary production)

2.6 kg CO₂/kg
2.2 kg CO₂/kg
2.7 kg CO₂/kg
2.3 kg CO₂/kg

Embodied Water

65 L/kg7.8 gal/lb
60 L/kg7.2 gal/lb
70 L/kg8.4 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

30%
40%
60%
35%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

115 kN·m/kg
90 kN·m/kg
103 kN·m/kg
138 kN·m/kg

Specific Stiffness (E / density)

26.3 MN·m/kg
26.3 MN·m/kg
26.9 MN·m/kg
26.3 MN·m/kg

Modulus of Resilience

1,195 kJ/m³
472 kJ/m³
595 kJ/m³
1,976 kJ/m³

Thermal Diffusivity

8.4 mm²/s
8.9 mm²/s
6.8 mm²/s
9.2 mm²/s

Thermal Shock Resistance Index

11
9
8
14

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleP201.2344718HNAK80

Manufacturing and finishing

CapabilityNAK80P201.2344718H
Default conditionAnnealedAnnealedAnnealedPrehard
Relative cost$$ Standard$$$$$ Specialty$$ Standard$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in NAK80 and P20 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.