FabDigit

B1500HS vs AR400 and 2 more: properties

B1500HSAR400AR500A514

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

210 GPa30.5 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Poisson's Ratio

0.3
0.29
0.29
0.29

Tensile Strength (Ultimate)

570 MPa82.7 ksi
1,250 MPa181 ksi
1,650 MPa239 ksi
800 MPa116 ksi

Yield Strength (0.2% offset)

380 MPa55.1 ksi
1,050 MPa152 ksi
1,350 MPa196 ksi
760 MPa110 ksi

Elongation at Break

17%
11%
9%
19%

Shear Strength

380 MPa55.1 ksi
780 MPa113 ksi
1,000 MPa145 ksi
480 MPa69.6 ksi

Fatigue Strength (Endurance Limit)

260 MPa37.7 ksi
520 MPa75.4 ksi
700 MPa102 ksi
380 MPa55.1 ksi

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
30 J22.1 ft·lbf
35 J25.8 ft·lbf
75 J55.3 ft·lbf

Hardness, Brinell

170 HB
400 HB
500 HB
250 HB

Hardness, Rockwell B

87 HRB
100 HRB

Hardness, Vickers

180 HV
420 HV
525 HV
262 HV

Reduction in Area

40%
30%
50%

Compressive Strength

1,100 MPa160 ksi
1,400 MPa203 ksi
760 MPa110 ksi

Fracture Toughness (K_IC)

70 MPa·√m63.7 ksi·√in
50 MPa·√m45.5 ksi·√in
120 MPa·√m109 ksi·√in

Hardness, Rockwell C

43 HRC
50 HRC
24 HRC

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,490°C2,714 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,425°C2,597 °F

Liquidus Temperature

1,520°C2,768 °F
1,500°C2,732 °F
1,500°C2,732 °F
1,510°C2,750 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

34 W/m·K19.6 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F
40 W/m·K23.1 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

12.5 µm/m·K6.9 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

350°C662 °F
250°C482 °F
250°C482 °F
400°C752 °F

Min Service Temperature

-40°C-40 °F
-20°C-4 °F
-40°C-40 °F
-45°C-49 °F

Same in both: Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Conductivity

8 % IACS
8 % IACS
7.5 % IACS
7 % IACS

Electrical Resistivity

2.1×10⁻⁷ Ω·m8.27 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.62 V
-0.6 V

Corrosion Resistance

12 / 100
12 / 100
13 / 100
16 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
22 / 100
12 / 100
38 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
20%
10%
40%

Weldability

70 / 100
55 / 100
45 / 100
55 / 100

Formability (cold)

65 / 100
25 / 100
15 / 100
30 / 100

Brazeability / Solderability

55 / 100
20 / 100
40 / 100

Polishability

45 / 100
55 / 100
55 / 100
50 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

32 MJ/kg13,758 BTU/lb
28 MJ/kg12,038 BTU/lb
30 MJ/kg12,898 BTU/lb
31 MJ/kg13,328 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

45 L/kg5.4 gal/lb
45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

20%
25%
25%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

73 kN·m/kg
159 kN·m/kg
210 kN·m/kg
102 kN·m/kg

Specific Stiffness (E / density)

26.8 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

344 kJ/m³
2,689 kJ/m³
4,445 kJ/m³
1,409 kJ/m³

Thermal Diffusivity

9.2 mm²/s
11.4 mm²/s
10.8 mm²/s
11.4 mm²/s

Thermal Shock Resistance Index

7
21
27
14

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleAR400AR500A514B1500HS

Manufacturing and finishing

CapabilityB1500HSAR400AR500A514
CNC machiningYesYesYes
Default conditionCRQ&TQ&TQ&T
Relative cost$$ Standard$$$ Premium$$$$ High$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrNYesYesYes
AlTiNYesYesYes
CVD Al2O3YesYesYes
CVD TiCNYesYesYes
CVD TiNYesYesYes
CrNYesYesYes
DLCYesYesYes
HVOF CoatingYesYesYes
MoS2YesYesYes
Multilayer CVDYesYesYes
TiAlNYesYesYes
TiB2YesYesYes
TiCNYesYesYes
TiNYesYesYes
WC/CYesYesYes
ZrNYesYesYes

Both are offered for Sheet metal. They share 22 finishes: Black Oxide, Cerakote, Chrome Plating, Copper Plating, E-Coating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Hot-Dip Galvanizing, Manganese Phosphate, Nickel Plating and 10 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in B1500HS and AR400 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.