FabDigit

4135 vs 4130 and 2 more: properties

4135413040Cr25CrMo4

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
205 GPa29.7 Msi
211 GPa30.6 Msi
210 GPa30.5 Msi

Shear Modulus

80 GPa11.6 Msi
80 GPa11.6 Msi
81 GPa11.7 Msi
80 GPa11.6 Msi

Tensile Strength (Ultimate)

700 MPa102 ksi
700 MPa102 ksi
720 MPa104 ksi
870 MPa126 ksi

Yield Strength (0.2% offset)

460 MPa66.7 ksi
440 MPa63.8 ksi
430 MPa62.4 ksi
650 MPa94.3 ksi

Elongation at Break

20%
22%
16%
16%

Reduction in Area

50%
50%
45%
50%

Shear Strength

430 MPa62.4 ksi
440 MPa63.8 ksi
430 MPa62.4 ksi
520 MPa75.4 ksi

Fatigue Strength (Endurance Limit)

320 MPa46.4 ksi
330 MPa47.9 ksi
330 MPa47.9 ksi
450 MPa65.3 ksi

Fracture Toughness (K_IC)

75 MPa·√m68.3 ksi·√in
110 MPa·√m100 ksi·√in
55 MPa·√m50.1 ksi·√in
90 MPa·√m81.9 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
55 J40.6 ft·lbf
40 J29.5 ft·lbf
60 J44.3 ft·lbf

Hardness, Brinell

200 HB
210 HB
210 HB
270 HB

Hardness, Rockwell B

93 HRB
95 HRB
94 HRB

Hardness, Vickers

210 HV
228 HV
285 HV

Compressive Strength

480 MPa69.6 ksi
430 MPa62.4 ksi
660 MPa95.7 ksi

Hardness, Rockwell C

16 HRC
28 HRC

Same in both: Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,416°C2,581 °F
1,432°C2,610 °F
1,425°C2,597 °F
1,420°C2,588 °F

Liquidus Temperature

1,480°C2,696 °F
1,510°C2,750 °F
1,495°C2,723 °F
1,500°C2,732 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

42 W/m·K24.3 BTU/hr·ft·°F
42.7 W/m·K24.7 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Specific Heat Capacity

477 J/kg·K0.11 BTU/lb·°F
477 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
460 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.5 µm/m·K6.9 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F

Latent Heat of Fusion

247 J/g106 BTU/lb
272 J/g117 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
400°C752 °F
500°C932 °F

Min Service Temperature

-40°C-40 °F
-50°C-58 °F
-30°C-22 °F
-40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.8 % IACS
7.7 % IACS
8 % IACS
7.8 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.23×10⁻⁷ Ω·m8.78 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.61 V
-0.6 V

Corrosion Resistance

12 / 100
14 / 100
12 / 100
13 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

58 / 100
55 / 100
55 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

62%
60%
60%
60%

Weldability

45 / 100
65 / 100
45 / 100
65 / 100

Formability (cold)

45 / 100
45 / 100
40 / 100
45 / 100

Brazeability / Solderability

60 / 100
70 / 100
55 / 100
60 / 100

Polishability

65 / 100
60 / 100
60 / 100
65 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

34 MJ/kg14,617 BTU/lb
30 MJ/kg12,898 BTU/lb
26 MJ/kg11,178 BTU/lb
31 MJ/kg13,328 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.3 kg CO₂/kg
2 kg CO₂/kg
2.2 kg CO₂/kg

Embodied Water

45 L/kg5.4 gal/lb
45 L/kg5.4 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

25%
30%
35%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

89 kN·m/kg
89 kN·m/kg
92 kN·m/kg
111 kN·m/kg

Specific Stiffness (E / density)

26.1 MN·m/kg
26.1 MN·m/kg
26.9 MN·m/kg
26.8 MN·m/kg

Modulus of Resilience

516 kJ/m³
472 kJ/m³
438 kJ/m³
1,006 kJ/m³

Thermal Diffusivity

11.2 mm²/s
11.4 mm²/s
11.9 mm²/s
11.6 mm²/s

Thermal Shock Resistance Index

12
12
12
14

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale413040Cr25CrMo44135

Manufacturing and finishing

Capability4135413040Cr25CrMo4
Default conditionHRHRHRQ&T
Relative cost$$ Standard$$ Standard$$ Standard$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 4135 and 4130 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.