FabDigit

34CrAlMo5-10 vs SACM645 and 2 more: properties

34CrAlMo5-10SACM64538CrMoAlA41CrAlMo7-10

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

210 GPa30.5 Msi
207 GPa30 Msi
210 GPa30.5 Msi
210 GPa30.5 Msi

Shear Modulus

81 GPa11.7 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi
81 GPa11.7 Msi

Tensile Strength (Ultimate)

900 MPa131 ksi
950 MPa138 ksi
1,030 MPa149 ksi
1,050 MPa152 ksi

Yield Strength (0.2% offset)

720 MPa104 ksi
780 MPa113 ksi
880 MPa128 ksi
800 MPa116 ksi

Elongation at Break

14%
17%
16%
14%

Reduction in Area

48%
55%
55%
50%

Compressive Strength

730 MPa106 ksi
790 MPa115 ksi
900 MPa131 ksi
820 MPa119 ksi

Shear Strength

550 MPa79.8 ksi
570 MPa82.7 ksi
640 MPa92.8 ksi
630 MPa91.4 ksi

Fatigue Strength (Endurance Limit)

430 MPa62.4 ksi
430 MPa62.4 ksi
470 MPa68.2 ksi
480 MPa69.6 ksi

Fracture Toughness (K_IC)

75 MPa·√m68.3 ksi·√in
70 MPa·√m63.7 ksi·√in
70 MPa·√m63.7 ksi·√in
70 MPa·√m63.7 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
75 J55.3 ft·lbf
80 J59 ft·lbf
45 J33.2 ft·lbf

Hardness, Brinell

280 HB
270 HB
310 HB
320 HB

Hardness, Rockwell C

29 HRC
28 HRC
32 HRC
34 HRC

Hardness, Vickers

295 HV
285 HV
325 HV
335 HV

Same in both: Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Density

7.8 g/cm³0.28 lb/in³
7.8 g/cm³0.28 lb/in³
7.8 g/cm³0.28 lb/in³
7.75 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,420°C2,588 °F
1,425°C2,597 °F
1,420°C2,588 °F
1,420°C2,588 °F

Same in both: Liquidus Temperature 1,490°C2,714 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

34 W/m·K19.6 BTU/hr·ft·°F
36 W/m·K20.8 BTU/hr·ft·°F
33 W/m·K19.1 BTU/hr·ft·°F
34 W/m·K19.6 BTU/hr·ft·°F

Specific Heat Capacity

460 J/kg·K0.11 BTU/lb·°F
465 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
460 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

500°C932 °F
450°C842 °F
500°C932 °F
500°C932 °F

Same in both: Min Service Temperature -40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

8 % IACS
7.5 % IACS
7.8 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.5×10⁻⁷ Ω·m9.84 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

12 / 100
15 / 100
12 / 100
15 / 100

Same in both: Galvanic Potential (seawater, vs SCE) -0.6 V

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
42 / 100
45 / 100
40 / 100

Machinability Rating (AISI 1212 = 100 %)

50%
45%
55%
45%

Weldability

20 / 100
18 / 100
20 / 100
15 / 100

Formability (cold)

25 / 100
25 / 100
20 / 100
15 / 100

Polishability

65 / 100
60 / 100
70 / 100
65 / 100

Brazeability / Solderability

40 / 100
35 / 100
30 / 100

Castability

25 / 100
20 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

31 MJ/kg13,328 BTU/lb
34 MJ/kg14,617 BTU/lb
34 MJ/kg14,617 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
2.5 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg

Embodied Water

55 L/kg6.6 gal/lb
55 L/kg6.6 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

30%
28%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

115 kN·m/kg
122 kN·m/kg
132 kN·m/kg
135 kN·m/kg

Specific Stiffness (E / density)

26.9 MN·m/kg
26.5 MN·m/kg
26.9 MN·m/kg
27.1 MN·m/kg

Modulus of Resilience

1,234 kJ/m³
1,470 kJ/m³
1,844 kJ/m³
1,524 kJ/m³

Thermal Diffusivity

9.5 mm²/s
9.9 mm²/s
9 mm²/s
9.5 mm²/s

Thermal Shock Resistance Index

12
14
14
15

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSACM64538CrMoAlA34CrAlMo5-1041CrAlMo7-10

Manufacturing and finishing

Capability34CrAlMo5-10SACM64538CrMoAlA41CrAlMo7-10
CNC machiningYesYes
Sheet metalYesYes
Default conditionQ&TQ&T
Relative cost$$ Standard$$ Standard$$ Standard$ Budget
Min. machined wall0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µm
AlCrNYesYes
AlTiNYesYes
Black OxideYesYes
CVD Al2O3YesYes
CVD TiCNYesYes
CVD TiNYesYes
CerakoteYesYes
Chrome PlatingYesYes
CrNYesYes
DLCYesYes
E-CoatingYesYes
HVOF CoatingYesYes
Hot-Dip GalvanizingYesYes
MoS2YesYes
Multilayer CVDYesYes
Nickel PlatingYesYes
PTFE CoatingYesYes
PaintingYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.