1006 vs 1008 and 2 more: properties

1006100810101012

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
200 GPa29 Msi
200 GPa29 Msi
205 GPa29.7 Msi

Tensile Strength (Ultimate)

300 MPa43.5 ksi
300 MPa43.5 ksi
325 MPa47.1 ksi
330 MPa47.9 ksi

Yield Strength (0.2% offset)

170 MPa24.7 ksi
175 MPa25.4 ksi
180 MPa26.1 ksi
185 MPa26.8 ksi

Elongation at Break

30%
30%
28%
28%

Reduction in Area

55%
55%
50%
55%

Shear Strength

200 MPa29 ksi
185 MPa26.8 ksi
220 MPa31.9 ksi
220 MPa31.9 ksi

Fatigue Strength (Endurance Limit)

150 MPa21.8 ksi
150 MPa21.8 ksi
160 MPa23.2 ksi
165 MPa23.9 ksi

Fracture Toughness (K_IC)

130 MPa·√m118 ksi·√in
140 MPa·√m127 ksi·√in
110 MPa·√m100 ksi·√in

Charpy V-Notch Impact (RT)

120 J88.5 ft·lbf
90 J66.4 ft·lbf
95 J70.1 ft·lbf
70 J51.6 ft·lbf

Hardness, Brinell

86 HB
86 HB
95 HB
95 HB

Hardness, Rockwell B

41 HRB
45 HRB
55 HRB
55 HRB

Hardness, Vickers

90 HV
100 HV

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,515°C2,759 °F
1,495°C2,723 °F
1,495°C2,723 °F
1,495°C2,723 °F

Liquidus Temperature

1,535°C2,795 °F
1,530°C2,786 °F
1,525°C2,777 °F
1,525°C2,777 °F

Same in both: Density 7.87 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

65 W/m·K37.6 BTU/hr·ft·°F
60 W/m·K34.7 BTU/hr·ft·°F
49.8 W/m·K28.8 BTU/hr·ft·°F
51.9 W/m·K30 BTU/hr·ft·°F

Specific Heat Capacity

481 J/kg·K0.11 BTU/lb·°F
481 J/kg·K0.11 BTU/lb·°F
448 J/kg·K0.11 BTU/lb·°F
486 J/kg·K0.12 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12 µm/m·K6.7 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12 µm/m·K6.7 µin/in·°F

Latent Heat of Fusion

247 J/g106 BTU/lb
247 J/g106 BTU/lb
247 J/g106 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
425°C797 °F
400°C752 °F
400°C752 °F

Min Service Temperature

-30°C-22 °F
-30°C-22 °F
-30°C-22 °F
-20°C-4 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

12 % IACS
11.5 % IACS
12 % IACS
10.8 % IACS

Electrical Resistivity

1.43×10⁻⁷ Ω·m5.63 µΩ·in
1.5×10⁻⁷ Ω·m5.91 µΩ·in
1.43×10⁻⁷ Ω·m5.63 µΩ·in
1.6×10⁻⁷ Ω·m6.3 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.65 V
-0.65 V
-0.61 V
-0.62 V

Same in both: Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
48 / 100
42 / 100
50 / 100

Machinability Rating (AISI 1212 = 100 %)

50%
45%
55%
55%

Weldability

97 / 100
95 / 100
95 / 100
95 / 100

Formability (cold)

95 / 100
85 / 100
90 / 100
85 / 100

Castability

35 / 100

Brazeability / Solderability

80 / 100
80 / 100
80 / 100
85 / 100

Polishability

45 / 100
50 / 100
40 / 100
45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

25 MJ/kg10,748 BTU/lb
25 MJ/kg10,748 BTU/lb
24 MJ/kg10,318 BTU/lb
25 MJ/kg10,748 BTU/lb

Embodied Carbon (primary production)

2.1 kg CO₂/kg
1.9 kg CO₂/kg
1.9 kg CO₂/kg
1.9 kg CO₂/kg

Embodied Water

55 L/kg6.6 gal/lb
40 L/kg4.8 gal/lb
35 L/kg4.2 gal/lb
40 L/kg4.8 gal/lb

Typical Recycled Content

28%
25%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

38 kN·m/kg
38 kN·m/kg
41 kN·m/kg
42 kN·m/kg

Specific Stiffness (E / density)

26 MN·m/kg
25.4 MN·m/kg
25.4 MN·m/kg
26 MN·m/kg

Modulus of Resilience

70 kJ/m³
77 kJ/m³
81 kJ/m³
83 kJ/m³

Thermal Diffusivity

17.2 mm²/s
15.9 mm²/s
14.1 mm²/s
13.6 mm²/s

Thermal Shock Resistance Index

8
7
7
7

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale1006100810101012

Manufacturing and finishing

Capability1006100810101012
CNC machiningYesYes
Default conditionHRHRHRHR
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µm
AlCrNYesYes
AlTiNYesYes
CVD Al2O3YesYes
CVD TiCNYesYes
CVD TiNYesYes
CrNYesYes
DLCYesYes
HVOF CoatingYesYes
MoS2YesYes
Multilayer CVDYesYes
TiAlNYesYes
TiB2YesYes
TiCNYesYes
TiNYesYes
WC/CYesYes
ZrNYesYes

Both are offered for Sheet metal. They share 22 finishes: Black Oxide, Cerakote, Chrome Plating, Copper Plating, E-Coating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Hot-Dip Galvanizing, Manganese Phosphate, Nickel Plating and 10 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 1006 and 1008 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.