FabDigit

G7 vs G5 and 2 more: properties

G7G5G11G10-ESD

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

14 GPa2 Msi
17 GPa2.5 Msi
22 GPa3.2 Msi
20 GPa2.9 Msi

Poisson's Ratio

0.17
0.17
0.13
0.15

Tensile Strength (Ultimate)

170 MPa24.7 ksi
220 MPa31.9 ksi
340 MPa49.3 ksi
300 MPa43.5 ksi

Compressive Strength

240 MPa34.8 ksi
415 MPa60.2 ksi
450 MPa65.3 ksi
450 MPa65.3 ksi

Compressive Modulus

12 GPa1.7 Msi
16 GPa2.3 Msi
20 GPa2.9 Msi
18 GPa2.6 Msi

Flexural Strength

172 MPa24.9 ksi
310 MPa45 ksi
450 MPa65.3 ksi
440 MPa63.8 ksi

Flexural Modulus

13 GPa1.9 Msi
18 GPa2.6 Msi
22 GPa3.2 Msi
19 GPa2.8 Msi

Shear Strength

95 MPa13.8 ksi
125 MPa18.1 ksi
140 MPa20.3 ksi
130 MPa18.9 ksi

Izod Impact, Notched

320 J/m6 ft·lbf/in
550 J/m10.3 ft·lbf/in
400 J/m7.5 ft·lbf/in
480 J/m9 ft·lbf/in

Hardness, Rockwell M

100 HRM
115 HRM
110 HRM
110 HRM

Shear Modulus

6 GPa0.87 Msi
5.5 GPa0.8 Msi
5.5 GPa0.8 Msi

Elongation at Break

1.5%
1.8%
2%

Fracture Toughness (K_IC)

12 MPa·√m10.9 ksi·√in
20 MPa·√m18.2 ksi·√in
25 MPa·√m22.8 ksi·√in

Hardness, Shore D

88 Shore D

Hardness, Rockwell R

125 HRR

Physical

Density and transition temperatures.

Density

1.8 g/cm³0.07 lb/in³
1.95 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³

Water Absorption (24 h)

0.2%
0.9%
0.1%
0.12%

Water Absorption (Saturation)

2%
0.35%
0.5%

Glass Transition (Tg)

150°C302 °F
120°C248 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.3 W/m·K0.17 BTU/hr·ft·°F
0.35 W/m·K0.2 BTU/hr·ft·°F
0.33 W/m·K0.19 BTU/hr·ft·°F
0.3 W/m·K0.17 BTU/hr·ft·°F

Specific Heat Capacity

1,000 J/kg·K0.24 BTU/lb·°F
1,100 J/kg·K0.26 BTU/lb·°F
1,100 J/kg·K0.26 BTU/lb·°F
1,100 J/kg·K0.26 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12 µm/m·K6.7 µin/in·°F
14 µm/m·K7.8 µin/in·°F
14 µm/m·K7.8 µin/in·°F
14 µm/m·K7.8 µin/in·°F

Max Service Temperature (continuous)

220°C428 °F
150°C302 °F
180°C356 °F
130°C266 °F

Min Service Temperature

-60°C-76 °F
-60°C-76 °F
-196°C-321 °F
-60°C-76 °F

Limiting Oxygen Index

40%
45%
22%
23%

Max Service Temperature (short-term)

260°C500 °F
200°C392 °F
220°C428 °F
155°C311 °F

Heat Deflection Temp. @ 1.8 MPa

200°C392 °F
200°C392 °F
200°C392 °F

Heat Deflection Temp. @ 0.45 MPa

215°C419 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10⁸ Ω·m3.94×10¹⁵ µΩ·in

Dielectric Strength

15 kV/mm381 V/mil
15 kV/mm381 V/mil
16 kV/mm406 V/mil

Dielectric Constant (1 MHz)

4.2
7.5
5.2

Dissipation Factor (1 MHz)

0.003
0.03
0.02

Volume Resistivity

1×10¹³ Ω·cm
1×10¹³ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁰ Ω·cm

Surface Resistivity

1×10¹² Ω
1×10¹² Ω
1×10¹³ Ω
1×10⁷ Ω

Comparative Tracking Index (CTI)

600 V
600 V
200 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

80 / 100
58 / 100
88 / 100
85 / 100

UV / Weathering Resistance

75 / 100
45 / 100
45 / 100
40 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

35 / 100
25 / 100
45 / 100
38 / 100

Polishability

25 / 100
30 / 100
30 / 100
25 / 100

Weldability

0 / 100
0 / 100
0 / 100

Formability (cold)

5 / 100
3 / 100
3 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

110 MJ/kg47,292 BTU/lb
75 MJ/kg32,244 BTU/lb
110 MJ/kg47,292 BTU/lb
120 MJ/kg51,591 BTU/lb

Embodied Carbon (primary production)

7 kg CO₂/kg
4.5 kg CO₂/kg
7 kg CO₂/kg
7 kg CO₂/kg

Embodied Water

200 L/kg24 gal/lb
200 L/kg24 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

94 kN·m/kg
113 kN·m/kg
184 kN·m/kg
162 kN·m/kg

Specific Stiffness (E / density)

7.8 MN·m/kg
8.7 MN·m/kg
11.9 MN·m/kg
10.8 MN·m/kg

Thermal Diffusivity

0.2 mm²/s
0.2 mm²/s
0.2 mm²/s
0.1 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every composite grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

1101001,000510Density (g/cm³)Yield strength (MPa) — log scaleG11G7G5G10-ESD

Manufacturing and finishing

CapabilityG7G5G11G10-ESD
Default conditionSilicone MatrixMelamine MatrixEpoxy MatrixEpoxy Matrix
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$ Premium
Min. machined wall
Best machined surface

Both are offered for CNC machining and Sheet metal. Both take the same 1 finish: Painting.

Ready to make it?

Upload a CAD file and FabDigit prices the part in G7 and G5 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.