FabDigit

G10-ESD vs G11 and 2 more: properties

G10-ESDG11FR-4G10

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

20 GPa2.9 Msi
22 GPa3.2 Msi
22 GPa3.2 Msi
20 GPa2.9 Msi

Shear Modulus

5.5 GPa0.8 Msi
5.5 GPa0.8 Msi
4.5 GPa0.65 Msi
5 GPa0.73 Msi

Poisson's Ratio

0.15
0.13
0.14
0.14

Tensile Strength (Ultimate)

300 MPa43.5 ksi
340 MPa49.3 ksi
310 MPa45 ksi
310 MPa45 ksi

Elongation at Break

2%
1.8%
1.8%
1.8%

Compressive Strength

450 MPa65.3 ksi
450 MPa65.3 ksi
415 MPa60.2 ksi
480 MPa69.6 ksi

Compressive Modulus

18 GPa2.6 Msi
20 GPa2.9 Msi
18 GPa2.6 Msi
18 GPa2.6 Msi

Flexural Strength

440 MPa63.8 ksi
450 MPa65.3 ksi
415 MPa60.2 ksi
480 MPa69.6 ksi

Flexural Modulus

19 GPa2.8 Msi
22 GPa3.2 Msi
20 GPa2.9 Msi
20 GPa2.9 Msi

Shear Strength

130 MPa18.9 ksi
140 MPa20.3 ksi
130 MPa18.9 ksi
150 MPa21.8 ksi

Fracture Toughness (K_IC)

25 MPa·√m22.8 ksi·√in
20 MPa·√m18.2 ksi·√in
15 MPa·√m13.7 ksi·√in

Izod Impact, Notched

480 J/m9 ft·lbf/in
400 J/m7.5 ft·lbf/in
420 J/m7.9 ft·lbf/in
430 J/m8.1 ft·lbf/in

Hardness, Rockwell R

125 HRR

Hardness, Shore D

88 Shore D

Same in both: Hardness, Rockwell M 110 HRM

Physical

Density and transition temperatures.

Density

1.85 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³
1.8 g/cm³0.07 lb/in³

Glass Transition (Tg)

120°C248 °F
150°C302 °F
135°C275 °F
120°C248 °F

Water Absorption (24 h)

0.12%
0.1%
0.12%
0.15%

Water Absorption (Saturation)

0.5%
0.35%
0.35%
0.6%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.3 W/m·K0.17 BTU/hr·ft·°F
0.33 W/m·K0.19 BTU/hr·ft·°F
0.3 W/m·K0.17 BTU/hr·ft·°F
0.35 W/m·K0.2 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

14 µm/m·K7.8 µin/in·°F
14 µm/m·K7.8 µin/in·°F
16 µm/m·K8.9 µin/in·°F
14 µm/m·K7.8 µin/in·°F

Max Service Temperature (continuous)

130°C266 °F
180°C356 °F
130°C266 °F
130°C266 °F

Min Service Temperature

-60°C-76 °F
-196°C-321 °F
-50°C-58 °F
-60°C-76 °F

Heat Deflection Temp. @ 0.45 MPa

215°C419 °F

Heat Deflection Temp. @ 1.8 MPa

200°C392 °F
200°C392 °F

Limiting Oxygen Index

23%
22%
30%
22%

Max Service Temperature (short-term)

155°C311 °F
220°C428 °F
180°C356 °F
180°C356 °F

Same in both: Specific Heat Capacity 1,100 J/kg·K0.26 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10⁸ Ω·m3.94×10¹⁵ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Volume Resistivity

1×10¹⁰ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁴ Ω·cm

Surface Resistivity

1×10⁷ Ω
1×10¹³ Ω
1×10¹³ Ω
1×10¹³ Ω

Dielectric Strength

16 kV/mm406 V/mil
20 kV/mm508 V/mil
20 kV/mm508 V/mil

Dielectric Constant (1 MHz)

5.2
4.6
5

Dissipation Factor (1 MHz)

0.02
0.02
0.022

Comparative Tracking Index (CTI)

200 V
200 V
200 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

85 / 100
88 / 100
85 / 100
85 / 100

UV / Weathering Resistance

40 / 100
45 / 100
40 / 100
35 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

38 / 100
45 / 100
45 / 100
45 / 100

Weldability

0 / 100
0 / 100
0 / 100

Formability (cold)

3 / 100
3 / 100
0 / 100

Polishability

25 / 100
30 / 100
30 / 100
25 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

120 MJ/kg51,591 BTU/lb
110 MJ/kg47,292 BTU/lb
95 MJ/kg40,843 BTU/lb
110 MJ/kg47,292 BTU/lb

Embodied Carbon (primary production)

7 kg CO₂/kg
7 kg CO₂/kg
6 kg CO₂/kg
7 kg CO₂/kg

Embodied Water

200 L/kg24 gal/lb
200 L/kg24 gal/lb
150 L/kg18 gal/lb
200 L/kg24 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

162 kN·m/kg
184 kN·m/kg
168 kN·m/kg
172 kN·m/kg

Specific Stiffness (E / density)

10.8 MN·m/kg
11.9 MN·m/kg
11.9 MN·m/kg
11.1 MN·m/kg

Thermal Diffusivity

0.1 mm²/s
0.2 mm²/s
0.1 mm²/s
0.2 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every composite grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

1101001,000510Density (g/cm³)Yield strength (MPa) — log scaleG11G10-ESDFR-4G10

Manufacturing and finishing

CapabilityG10-ESDG11FR-4G10
Default conditionEpoxy MatrixEpoxy MatrixEpoxy MatrixEpoxy Matrix
Relative cost$$$ Premium$$$ Premium$$ Standard$$$ Premium
Min. machined wall
Best machined surface

Both are offered for CNC machining and Sheet metal. Both take the same 1 finish: Painting.

Ready to make it?

Upload a CAD file and FabDigit prices the part in G10-ESD and G11 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.