FabDigit

G10 vs G11 and 2 more: properties

G10G11G10-ESDFR-4

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

20 GPa2.9 Msi
22 GPa3.2 Msi
20 GPa2.9 Msi
22 GPa3.2 Msi

Shear Modulus

5 GPa0.73 Msi
5.5 GPa0.8 Msi
5.5 GPa0.8 Msi
4.5 GPa0.65 Msi

Poisson's Ratio

0.14
0.13
0.15
0.14

Tensile Strength (Ultimate)

310 MPa45 ksi
340 MPa49.3 ksi
300 MPa43.5 ksi
310 MPa45 ksi

Elongation at Break

1.8%
1.8%
2%
1.8%

Compressive Strength

480 MPa69.6 ksi
450 MPa65.3 ksi
450 MPa65.3 ksi
415 MPa60.2 ksi

Compressive Modulus

18 GPa2.6 Msi
20 GPa2.9 Msi
18 GPa2.6 Msi
18 GPa2.6 Msi

Flexural Strength

480 MPa69.6 ksi
450 MPa65.3 ksi
440 MPa63.8 ksi
415 MPa60.2 ksi

Flexural Modulus

20 GPa2.9 Msi
22 GPa3.2 Msi
19 GPa2.8 Msi
20 GPa2.9 Msi

Shear Strength

150 MPa21.8 ksi
140 MPa20.3 ksi
130 MPa18.9 ksi
130 MPa18.9 ksi

Fracture Toughness (K_IC)

15 MPa·√m13.7 ksi·√in
20 MPa·√m18.2 ksi·√in
25 MPa·√m22.8 ksi·√in

Izod Impact, Notched

430 J/m8.1 ft·lbf/in
400 J/m7.5 ft·lbf/in
480 J/m9 ft·lbf/in
420 J/m7.9 ft·lbf/in

Hardness, Shore D

88 Shore D

Hardness, Rockwell R

125 HRR

Same in both: Hardness, Rockwell M 110 HRM

Physical

Density and transition temperatures.

Density

1.8 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³
1.85 g/cm³0.07 lb/in³

Glass Transition (Tg)

120°C248 °F
150°C302 °F
120°C248 °F
135°C275 °F

Water Absorption (24 h)

0.15%
0.1%
0.12%
0.12%

Water Absorption (Saturation)

0.6%
0.35%
0.5%
0.35%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.35 W/m·K0.2 BTU/hr·ft·°F
0.33 W/m·K0.19 BTU/hr·ft·°F
0.3 W/m·K0.17 BTU/hr·ft·°F
0.3 W/m·K0.17 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

14 µm/m·K7.8 µin/in·°F
14 µm/m·K7.8 µin/in·°F
14 µm/m·K7.8 µin/in·°F
16 µm/m·K8.9 µin/in·°F

Max Service Temperature (continuous)

130°C266 °F
180°C356 °F
130°C266 °F
130°C266 °F

Min Service Temperature

-60°C-76 °F
-196°C-321 °F
-60°C-76 °F
-50°C-58 °F

Limiting Oxygen Index

22%
22%
23%
30%

Max Service Temperature (short-term)

180°C356 °F
220°C428 °F
155°C311 °F
180°C356 °F

Heat Deflection Temp. @ 1.8 MPa

200°C392 °F
200°C392 °F

Heat Deflection Temp. @ 0.45 MPa

215°C419 °F

Same in both: Specific Heat Capacity 1,100 J/kg·K0.26 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10⁸ Ω·m3.94×10¹⁵ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Dielectric Strength

20 kV/mm508 V/mil
16 kV/mm406 V/mil
20 kV/mm508 V/mil

Dielectric Constant (1 MHz)

5
5.2
4.6

Dissipation Factor (1 MHz)

0.022
0.02
0.02

Volume Resistivity

1×10¹⁴ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁰ Ω·cm
1×10¹⁴ Ω·cm

Surface Resistivity

1×10¹³ Ω
1×10¹³ Ω
1×10⁷ Ω
1×10¹³ Ω

Comparative Tracking Index (CTI)

200 V
200 V
200 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

85 / 100
88 / 100
85 / 100
85 / 100

UV / Weathering Resistance

35 / 100
45 / 100
40 / 100
40 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
45 / 100
38 / 100
45 / 100

Weldability

0 / 100
0 / 100
0 / 100

Formability (cold)

0 / 100
3 / 100
3 / 100

Polishability

25 / 100
30 / 100
25 / 100
30 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

110 MJ/kg47,292 BTU/lb
110 MJ/kg47,292 BTU/lb
120 MJ/kg51,591 BTU/lb
95 MJ/kg40,843 BTU/lb

Embodied Carbon (primary production)

7 kg CO₂/kg
7 kg CO₂/kg
7 kg CO₂/kg
6 kg CO₂/kg

Embodied Water

200 L/kg24 gal/lb
200 L/kg24 gal/lb
200 L/kg24 gal/lb
150 L/kg18 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

172 kN·m/kg
184 kN·m/kg
162 kN·m/kg
168 kN·m/kg

Specific Stiffness (E / density)

11.1 MN·m/kg
11.9 MN·m/kg
10.8 MN·m/kg
11.9 MN·m/kg

Thermal Diffusivity

0.2 mm²/s
0.2 mm²/s
0.1 mm²/s
0.1 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every composite grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

1101001,000510Density (g/cm³)Yield strength (MPa) — log scaleG11G10-ESDFR-4G10

Manufacturing and finishing

CapabilityG10G11G10-ESDFR-4
Default conditionEpoxy MatrixEpoxy MatrixEpoxy MatrixEpoxy Matrix
Relative cost$$$ Premium$$$ Premium$$$ Premium$$ Standard
Min. machined wall
Best machined surface

Both are offered for CNC machining and Sheet metal. Both take the same 1 finish: Painting.

Ready to make it?

Upload a CAD file and FabDigit prices the part in G10 and G11 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.