Zircon vs Steatite and 2 more: properties

ZirconSteatiteCordieriteMullite

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

190 GPa27.6 Msi
100 GPa14.5 Msi
70 GPa10.2 Msi
150 GPa21.8 Msi

Shear Modulus

78 GPa11.3 Msi
40 GPa5.8 Msi
28 GPa4.1 Msi
60 GPa8.7 Msi

Bulk Modulus

150 GPa21.8 Msi
67 GPa9.7 Msi
47 GPa6.8 Msi
145 GPa21 Msi

Tensile Strength (Ultimate)

80 MPa11.6 ksi
60 MPa8.7 ksi
25 MPa3.6 ksi
80 MPa11.6 ksi

Compressive Strength

1,200 MPa174 ksi
700 MPa102 ksi
350 MPa50.8 ksi
700 MPa102 ksi

Flexural Strength

180 MPa26.1 ksi
130 MPa18.9 ksi
70 MPa10.2 ksi
170 MPa24.7 ksi

Fracture Toughness (K_IC)

2.5 MPa·√m2.3 ksi·√in
1.5 MPa·√m1.4 ksi·√in
1.5 MPa·√m1.4 ksi·√in
2.2 MPa·√m2 ksi·√in

Hardness, Vickers

1,150 HV
650 HV
700 HV
1,100 HV

Hardness, Knoop

1,100 HK
600 HK
—
1,000 HK

Hardness, Mohs

7.5
7
7
7.5

Elongation at Break

—
0%
—
0%

Shear Strength

—
—
—
115 MPa16.7 ksi

Same in both: Poisson's Ratio 0.25

Physical

Density and transition temperatures.

Density

3.7 g/cm³0.13 lb/in³
2.8 g/cm³0.1 lb/in³
2.3 g/cm³0.08 lb/in³
2.9 g/cm³0.1 lb/in³

Melting Point (Solidus)

1,687°C3,069 °F
1,450°C2,642 °F
1,465°C2,669 °F
1,840°C3,344 °F

Refractive Index

1.95
—
—
1.64

Porosity

0.2%
0%
8%
1%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

4.5 W/m·K2.6 BTU/hr·ft·°F
2.5 W/m·K1.4 BTU/hr·ft·°F
2.5 W/m·K1.4 BTU/hr·ft·°F
5 W/m·K2.9 BTU/hr·ft·°F

Specific Heat Capacity

560 J/kg·K0.13 BTU/lb·°F
800 J/kg·K0.19 BTU/lb·°F
800 J/kg·K0.19 BTU/lb·°F
880 J/kg·K0.21 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

4.2 µm/m·K2.3 µin/in·°F
8 µm/m·K4.4 µin/in·°F
2 µm/m·K1.1 µin/in·°F
4.5 µm/m·K2.5 µin/in·°F

Max Service Temperature (continuous)

1,500°C2,732 °F
1,000°C1,832 °F
1,250°C2,282 °F
1,550°C2,822 °F

Same in both: Min Service Temperature -200°C-328 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Dielectric Strength

12 kV/mm305 V/mil
12 kV/mm305 V/mil
10 kV/mm254 V/mil
12 kV/mm305 V/mil

Dielectric Constant (1 MHz)

9
6
5
6.5

Dissipation Factor (1 MHz)

0.001
0.0012
0.004
0.003

Volume Resistivity

1×10¹³ Ω·cm
1×10¹⁴ Ω·cm
1×10¹³ Ω·cm
1×10¹⁴ Ω·cm

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

88 / 100
85 / 100
70 / 100
80 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

5 / 100
8 / 100
20 / 100
5 / 100

Polishability

80 / 100
60 / 100
35 / 100
60 / 100

Sintering / Firing Temperature

1,600°C2,912 °F
1,300°C2,372 °F
1,350°C2,462 °F
1,650°C3,002 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

40 MJ/kg17,197 BTU/lb
27 MJ/kg11,608 BTU/lb
30 MJ/kg12,898 BTU/lb
45 MJ/kg19,347 BTU/lb

Embodied Carbon (primary production)

3 kg CO₂/kg
1.9 kg CO₂/kg
2.2 kg CO₂/kg
3.2 kg CO₂/kg

Embodied Water

30 L/kg3.6 gal/lb
45 L/kg5.4 gal/lb
20 L/kg2.4 gal/lb
90 L/kg10.8 gal/lb

Typical Recycled Content

3%
2%
5%
5%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

22 kN·m/kg
21 kN·m/kg
11 kN·m/kg
28 kN·m/kg

Specific Stiffness (E / density)

51.4 MN·m/kg
35.7 MN·m/kg
30.4 MN·m/kg
51.7 MN·m/kg

Thermal Diffusivity

2.2 mm²/s
1.1 mm²/s
1.4 mm²/s
2 mm²/s

Thermal Shock Resistance Index

0
0
0
1

Strength versus weight

Yield strength against density for every ceramic grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

501002005001,000234567Density (g/cm³)Yield strength (MPa) — log scaleSteatiteCordierite

Manufacturing and finishing

CapabilityZirconSteatiteCordieriteMullite
Default condition————
Relative cost$$ Standard$$$$ High$$$$ High$$$ Premium
Min. machined wall————
Best machined surface————

Ready to make it?

Upload a CAD file and FabDigit prices the part in Zircon and Steatite side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.