FabDigit

TiN vs Silicon Nitride and 2 more: properties

TiNSilicon NitrideBoron NitrideAlN

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

250 GPa36.3 Msi
310 GPa45 Msi
45 GPa6.5 Msi
320 GPa46.4 Msi

Bulk Modulus

290 GPa42.1 Msi
222 GPa32.2 Msi
36 GPa5.2 Msi
200 GPa29 Msi

Poisson's Ratio

0.25
0.27
0.2
0.24

Compressive Strength

1,400 MPa203 ksi
3,000 MPa435 ksi
90 MPa13.1 ksi
2,100 MPa305 ksi

Flexural Strength

350 MPa50.8 ksi
800 MPa116 ksi
55 MPa8 ksi
330 MPa47.9 ksi

Fracture Toughness (K_IC)

4 MPa·√m3.6 ksi·√in
6.5 MPa·√m5.9 ksi·√in
1 MPa·√m0.91 ksi·√in
2.7 MPa·√m2.5 ksi·√in

Hardness, Vickers

1,900 HV
1,500 HV
1,100 HV

Hardness, Knoop

1,800 HK
1,500 HK
1,200 HK

Hardness, Mohs

9
9
2
7.5

Shear Modulus

122 GPa17.7 Msi
18 GPa2.6 Msi
130 GPa18.9 Msi

Tensile Strength (Ultimate)

450 MPa65.3 ksi
35 MPa5.1 ksi
200 MPa29 ksi

Elongation at Break

0%

Physical

Density and transition temperatures.

Density

5.22 g/cm³0.19 lb/in³
3.22 g/cm³0.12 lb/in³
2 g/cm³0.07 lb/in³
3.26 g/cm³0.12 lb/in³

Melting Point (Solidus)

2,950°C5,342 °F
1,900°C3,452 °F
2,973°C5,383 °F
2,200°C3,992 °F

Porosity

2%
0.5%
8%
0.2%

Light Transmission

0%

Refractive Index

1.75
2.15

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

29 W/m·K16.8 BTU/hr·ft·°F
25 W/m·K14.4 BTU/hr·ft·°F
33 W/m·K19.1 BTU/hr·ft·°F
180 W/m·K104 BTU/hr·ft·°F

Specific Heat Capacity

600 J/kg·K0.14 BTU/lb·°F
700 J/kg·K0.17 BTU/lb·°F
800 J/kg·K0.19 BTU/lb·°F
740 J/kg·K0.18 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

9.4 µm/m·K5.2 µin/in·°F
3.2 µm/m·K1.8 µin/in·°F
2 µm/m·K1.1 µin/in·°F
4.4 µm/m·K2.4 µin/in·°F

Max Service Temperature (continuous)

600°C1,112 °F
1,200°C2,192 °F
1,000°C1,832 °F
900°C1,652 °F

Min Service Temperature

-250°C-418 °F
-269°C-452 °F
-200°C-328 °F
-200°C-328 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

3×10⁻⁷ Ω·m11.8 µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹³ Ω·m3.94×10²⁰ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Volume Resistivity

3×10⁻⁵ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁵ Ω·cm
1×10¹⁴ Ω·cm

Dielectric Strength

15 kV/mm381 V/mil
40 kV/mm1,016 V/mil
17 kV/mm432 V/mil

Dielectric Constant (1 MHz)

8
4.1
8.8

Dissipation Factor (1 MHz)

0.001
4×10⁻⁴
5×10⁻⁴

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

75 / 100
92 / 100
70 / 100
85 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

8 / 100
5 / 100
85 / 100
5 / 100

Polishability

85 / 100
92 / 100
25 / 100
85 / 100

Sintering / Firing Temperature

1,800°C3,272 °F
1,750°C3,182 °F
1,800°C3,272 °F
1,800°C3,272 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

200 MJ/kg85,985 BTU/lb
170 MJ/kg73,087 BTU/lb
250 MJ/kg107,481 BTU/lb
280 MJ/kg120,378 BTU/lb

Embodied Carbon (primary production)

15 kg CO₂/kg
12 kg CO₂/kg
20 kg CO₂/kg
22 kg CO₂/kg

Embodied Water

220 L/kg26.4 gal/lb
120 L/kg14.4 gal/lb
300 L/kg35.9 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Stiffness (E / density)

47.9 MN·m/kg
96.3 MN·m/kg
22.5 MN·m/kg
98.2 MN·m/kg

Thermal Diffusivity

9.3 mm²/s
11.1 mm²/s
20.6 mm²/s
74.6 mm²/s

Strength versus weight

Yield strength against density for every ceramic grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

501002005001,000234567Density (g/cm³)Yield strength (MPa) — log scaleSilicon NitrideBoron Nitride

Manufacturing and finishing

CapabilityTiNSilicon NitrideBoron NitrideAlN
Default condition
Relative cost$$$$ High$$$$ High$$$$ High$$$$ High
Min. machined wall
Best machined surface