A356 vs 319 and 2 more: properties

A356319355356

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

72.4 GPa10.5 Msi
74 GPa10.7 Msi
71 GPa10.3 Msi
72.4 GPa10.5 Msi

Shear Modulus

26.5 GPa3.8 Msi
27.5 GPa4 Msi
26.5 GPa3.8 Msi
27 GPa3.9 Msi

Bulk Modulus

70 GPa10.2 Msi
72 GPa10.4 Msi
69 GPa10 Msi
71 GPa10.3 Msi

Tensile Strength (Ultimate)

230 MPa33.4 ksi
186 MPa27 ksi
250 MPa36.3 ksi
262 MPa38 ksi

Yield Strength (0.2% offset)

165 MPa23.9 ksi
124 MPa18 ksi
180 MPa26.1 ksi
186 MPa27 ksi

Elongation at Break

4%
2%
3%
5%

Compressive Strength

175 MPa25.4 ksi
190 MPa27.6 ksi

Shear Strength

180 MPa26.1 ksi
150 MPa21.8 ksi
195 MPa28.3 ksi
179 MPa26 ksi

Fatigue Strength (Endurance Limit)

90 MPa13.1 ksi
69 MPa10 ksi
62 MPa9 ksi
90 MPa13.1 ksi

Fracture Toughness (K_IC)

20 MPa·√m18.2 ksi·√in
19 MPa·√m17.3 ksi·√in
20 MPa·√m18.2 ksi·√in
20 MPa·√m18.2 ksi·√in

Charpy V-Notch Impact (RT)

4 J3 ft·lbf
4 J3 ft·lbf
5 J3.7 ft·lbf

Hardness, Brinell

75 HB
70 HB
85 HB
80 HB

Hardness, Vickers

85 HV

Same in both: Poisson's Ratio 0.33

Physical

Density and transition temperatures.

Density

2.68 g/cm³0.1 lb/in³
2.79 g/cm³0.1 lb/in³
2.71 g/cm³0.1 lb/in³
2.67 g/cm³0.1 lb/in³

Melting Point (Solidus)

557°C1,035 °F
521°C970 °F
546°C1,015 °F
557°C1,035 °F

Liquidus Temperature

613°C1,135 °F
604°C1,119 °F
621°C1,150 °F
613°C1,135 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

151 W/m·K87.2 BTU/hr·ft·°F
109 W/m·K63 BTU/hr·ft·°F
151 W/m·K87.2 BTU/hr·ft·°F
151 W/m·K87.2 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

21.4 µm/m·K11.9 µin/in·°F
21.5 µm/m·K11.9 µin/in·°F
22.4 µm/m·K12.4 µin/in·°F
21.5 µm/m·K11.9 µin/in·°F

Max Service Temperature (continuous)

150°C302 °F
200°C392 °F
175°C347 °F
150°C302 °F

Same in both: Specific Heat Capacity 963 J/kg·K0.23 BTU/lb·°F · Latent Heat of Fusion 389 J/g167 BTU/lb · Min Service Temperature -196°C-321 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

39 % IACS
27 % IACS
36 % IACS
39 % IACS

Electrical Resistivity

4.42×10⁻⁸ Ω·m1.74 µΩ·in
6.4×10⁻⁸ Ω·m2.52 µΩ·in
4.8×10⁻⁸ Ω·m1.89 µΩ·in
4.4×10⁻⁸ Ω·m1.73 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.83 V
-0.78 V
-0.78 V
-0.83 V

Corrosion Resistance

68 / 100
35 / 100
45 / 100
62 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

68 / 100
72 / 100
62 / 100
70 / 100

Machinability Rating (AISI 1212 = 100 %)

80%
130%
60%
120%

Weldability

80 / 100
55 / 100
55 / 100
78 / 100

Formability (cold)

15 / 100
5 / 100
5 / 100
10 / 100

Castability

95 / 100
90 / 100
85 / 100
95 / 100

Brazeability / Solderability

40 / 100
25 / 100
25 / 100
30 / 100

Polishability

55 / 100
40 / 100
45 / 100
45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Carbon (primary production)

12 kg CO₂/kg
12 kg CO₂/kg
12 kg CO₂/kg
12.5 kg CO₂/kg

Embodied Water

1,150 L/kg138 gal/lb
1,200 L/kg144 gal/lb
1,100 L/kg132 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

50%
75%
80%
60%

Same in both: Embodied Energy (primary production) 200 MJ/kg85,985 BTU/lb

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

86 kN·m/kg
67 kN·m/kg
92 kN·m/kg
98 kN·m/kg

Specific Stiffness (E / density)

27 MN·m/kg
26.5 MN·m/kg
26.2 MN·m/kg
27.1 MN·m/kg

Modulus of Resilience

188 kJ/m³
104 kJ/m³
228 kJ/m³
239 kJ/m³

Thermal Diffusivity

58.5 mm²/s
40.6 mm²/s
57.9 mm²/s
58.7 mm²/s

Thermal Shock Resistance Index

22
13
24
25

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale319355356A356

Manufacturing and finishing

CapabilityA356319355356
Casting & forgingYes
Default condition
Relative cost$$ Standard$ Budget$ Budget$ Budget
Min. machined wall1 mm0.5 mm0.5 mm0.5 mm
Best machined surfaceRa 1.6 µmRa 0.8 µmRa 0.8 µmRa 0.8 µm

Both are offered for CNC machining. Both take the same 16 finishes: Anodizing Type II, Cerakote, Chem Film (Alodine), DLC, E-Coating, Electroless Nickel (EN), Electropolishing, Epoxy Coating, Gold Plating, Hard Anodize Type III w/ PTFE, Hard Anodizing Type III, Nickel Plating and 4 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in A356 and 319 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.