FabDigit

A20X vs 2024 and 2 more: properties

A20X202420142117

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

77 GPa11.2 Msi
73.1 GPa10.6 Msi
72.4 GPa10.5 Msi
70.3 GPa10.2 Msi

Shear Modulus

29 GPa4.2 Msi
28 GPa4.1 Msi
28 GPa4.1 Msi
26.5 GPa3.8 Msi

Bulk Modulus

73 GPa10.6 Msi
73 GPa10.6 Msi
71 GPa10.3 Msi
74 GPa10.7 Msi

Tensile Strength (Ultimate)

380 MPa55.1 ksi
483 MPa70.1 ksi
483 MPa70.1 ksi
295 MPa42.8 ksi

Yield Strength (0.2% offset)

240 MPa34.8 ksi
345 MPa50 ksi
414 MPa60 ksi
165 MPa23.9 ksi

Elongation at Break

12%
18%
13%
27%

Reduction in Area

15%

Compressive Strength

250 MPa36.3 ksi
350 MPa50.8 ksi
425 MPa61.6 ksi

Shear Strength

235 MPa34.1 ksi
283 MPa41 ksi
290 MPa42.1 ksi
195 MPa28.3 ksi

Fatigue Strength (Endurance Limit)

105 MPa15.2 ksi
138 MPa20 ksi
125 MPa18.1 ksi
95 MPa13.8 ksi

Fracture Toughness (K_IC)

28 MPa·√m25.5 ksi·√in
37 MPa·√m33.7 ksi·√in
24 MPa·√m21.8 ksi·√in

Charpy V-Notch Impact (RT)

10 J7.4 ft·lbf

Hardness, Brinell

95 HB
120 HB
135 HB
70 HB

Hardness, Rockwell B

58 HRB
75 HRB

Hardness, Vickers

105 HV
137 HV
145 HV

Same in both: Poisson's Ratio 0.33

Physical

Density and transition temperatures.

Density

2.83 g/cm³0.1 lb/in³
2.78 g/cm³0.1 lb/in³
2.8 g/cm³0.1 lb/in³
2.75 g/cm³0.1 lb/in³

Melting Point (Solidus)

545°C1,013 °F
502°C936 °F
507°C945 °F
554°C1,029 °F

Liquidus Temperature

645°C1,193 °F
638°C1,180 °F
638°C1,180 °F
650°C1,202 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

105 W/m·K60.7 BTU/hr·ft·°F
121 W/m·K69.9 BTU/hr·ft·°F
155 W/m·K89.6 BTU/hr·ft·°F
151 W/m·K87.2 BTU/hr·ft·°F

Specific Heat Capacity

870 J/kg·K0.21 BTU/lb·°F
875 J/kg·K0.21 BTU/lb·°F
864 J/kg·K0.21 BTU/lb·°F
864 J/kg·K0.21 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

22.3 µm/m·K12.4 µin/in·°F
22.9 µm/m·K12.7 µin/in·°F
22.5 µm/m·K12.5 µin/in·°F
23.8 µm/m·K13.2 µin/in·°F

Max Service Temperature (continuous)

150°C302 °F
150°C302 °F
150°C302 °F
120°C248 °F

Min Service Temperature

-196°C-321 °F
-196°C-321 °F
-200°C-328 °F
-200°C-328 °F

Same in both: Latent Heat of Fusion 390 J/g168 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

28 % IACS
30 % IACS
40 % IACS
40 % IACS

Electrical Resistivity

6.2×10⁻⁸ Ω·m2.44 µΩ·in
5.75×10⁻⁸ Ω·m2.26 µΩ·in
4.3×10⁻⁸ Ω·m1.69 µΩ·in
4.31×10⁻⁸ Ω·m1.7 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.65 V
-0.69 V
-0.78 V
-0.64 V

Corrosion Resistance

35 / 100
32 / 100
30 / 100
35 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

70 / 100
72 / 100
78 / 100
65 / 100

Machinability Rating (AISI 1212 = 100 %)

200%
70%
200%

Weldability

50 / 100
20 / 100
25 / 100
20 / 100

Formability (cold)

25 / 100
40 / 100
30 / 100
75 / 100

Castability

75 / 100
10 / 100
25 / 100

Brazeability / Solderability

25 / 100
15 / 100
15 / 100
15 / 100

Polishability

60 / 100
55 / 100
55 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

240 MJ/kg103,182 BTU/lb
200 MJ/kg85,985 BTU/lb
200 MJ/kg85,985 BTU/lb
155 MJ/kg66,638 BTU/lb

Embodied Carbon (primary production)

15 kg CO₂/kg
12.5 kg CO₂/kg
12.5 kg CO₂/kg
12 kg CO₂/kg

Embodied Water

1,200 L/kg144 gal/lb
1,100 L/kg132 gal/lb
1,100 L/kg132 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

5%
10%
20%
25%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

134 kN·m/kg
174 kN·m/kg
173 kN·m/kg
107 kN·m/kg

Specific Stiffness (E / density)

27.2 MN·m/kg
26.3 MN·m/kg
25.9 MN·m/kg
25.6 MN·m/kg

Modulus of Resilience

374 kJ/m³
814 kJ/m³
1,184 kJ/m³
194 kJ/m³

Thermal Diffusivity

42.6 mm²/s
49.7 mm²/s
64.1 mm²/s
63.6 mm²/s

Thermal Shock Resistance Index

23
35
46
27

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale201420242117A20X

Manufacturing and finishing

CapabilityA20X202420142117
3D printingYes
CNC machiningYesYesYes
Sheet metalYesYesYes
Default conditionAs PrintedT3
Relative cost$$$$$ Specialty$$$ Premium$$$ Premium$$$ Premium
Min. machined wall0.8 mm0.8 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
Anodized (Aluminum AM)Yes
Anodizing Type IIYesYesYes
CerakoteYesYesYes
Chem Film (Alodine)YesYesYes
DLCYesYesYes
E-CoatingYesYesYes
ElectropolishingYesYesYes
Hard Anodize Type III w/ PTFEYesYesYes
Hard Anodizing Type IIIYesYesYes
Nickel PlatingYesYesYes
PTFE CoatingYesYesYes
PaintingYesYesYes
Plated (Metal AM)Yes
Powder CoatingYesYesYes

They share 4 finishes: Electroless Nickel (EN), Epoxy Coating, Gold Plating, Silver Plating.

Ready to make it?

Upload a CAD file and FabDigit prices the part in A20X and 2024 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.