FabDigit

7475 vs 7075 and 2 more: properties

7475707570727003

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

71 GPa10.3 Msi
71.7 GPa10.4 Msi
69 GPa10 Msi
70 GPa10.2 Msi

Shear Modulus

27 GPa3.9 Msi
26.9 GPa3.9 Msi
26 GPa3.8 Msi
26.5 GPa3.8 Msi

Bulk Modulus

70 GPa10.2 Msi
70 GPa10.2 Msi
69 GPa10 Msi
71 GPa10.3 Msi

Tensile Strength (Ultimate)

490 MPa71.1 ksi
572 MPa83 ksi
55 MPa8 ksi
360 MPa52.2 ksi

Yield Strength (0.2% offset)

421 MPa61.1 ksi
503 MPa73 ksi
21 MPa3 ksi
315 MPa45.7 ksi

Elongation at Break

13%
11%
32%
11%

Compressive Strength

428 MPa62.1 ksi
505 MPa73.2 ksi
320 MPa46.4 ksi

Shear Strength

290 MPa42.1 ksi
331 MPa48 ksi
41 MPa5.9 ksi
210 MPa30.5 ksi

Fatigue Strength (Endurance Limit)

152 MPa22 ksi
159 MPa23.1 ksi
30 MPa4.4 ksi
130 MPa18.9 ksi

Fracture Toughness (K_IC)

66 MPa·√m60.1 ksi·√in
27 MPa·√m24.6 ksi·√in
28 MPa·√m25.5 ksi·√in

Hardness, Brinell

135 HB
150 HB
20 HB
105 HB

Reduction in Area

25%

Charpy V-Notch Impact (RT)

8 J5.9 ft·lbf

Hardness, Rockwell B

87 HRB

Hardness, Vickers

175 HV
112 HV

Same in both: Poisson's Ratio 0.33

Physical

Density and transition temperatures.

Density

2.81 g/cm³0.1 lb/in³
2.81 g/cm³0.1 lb/in³
2.72 g/cm³0.1 lb/in³
2.78 g/cm³0.1 lb/in³

Melting Point (Solidus)

477°C891 °F
477°C891 °F
640°C1,184 °F
605°C1,121 °F

Liquidus Temperature

635°C1,175 °F
635°C1,175 °F
657°C1,215 °F
645°C1,193 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

163 W/m·K94.2 BTU/hr·ft·°F
130 W/m·K75.1 BTU/hr·ft·°F
227 W/m·K131 BTU/hr·ft·°F
150 W/m·K86.7 BTU/hr·ft·°F

Specific Heat Capacity

864 J/kg·K0.21 BTU/lb·°F
960 J/kg·K0.23 BTU/lb·°F
900 J/kg·K0.21 BTU/lb·°F
875 J/kg·K0.21 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

22.7 µm/m·K12.6 µin/in·°F
23.6 µm/m·K13.1 µin/in·°F
23.6 µm/m·K13.1 µin/in·°F
23.2 µm/m·K12.9 µin/in·°F

Latent Heat of Fusion

390 J/g168 BTU/lb
395 J/g170 BTU/lb
395 J/g170 BTU/lb
390 J/g168 BTU/lb

Max Service Temperature (continuous)

150°C302 °F
120°C248 °F
150°C302 °F
120°C248 °F

Same in both: Min Service Temperature -196°C-321 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

40 % IACS
33 % IACS
60 % IACS
39 % IACS

Electrical Resistivity

4.31×10⁻⁸ Ω·m1.7 µΩ·in
5.15×10⁻⁸ Ω·m2.03 µΩ·in
2.87×10⁻⁸ Ω·m1.13 µΩ·in
4.4×10⁻⁸ Ω·m1.73 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.82 V
-0.83 V
-0.96 V
-0.86 V

Corrosion Resistance

50 / 100
35 / 100
72 / 100
55 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

72 / 100
78 / 100
30 / 100
65 / 100

Machinability Rating (AISI 1212 = 100 %)

70%
160%
30%
200%

Weldability

18 / 100
18 / 100
80 / 100
75 / 100

Formability (cold)

30 / 100
25 / 100
95 / 100
35 / 100

Castability

20 / 100

Brazeability / Solderability

10 / 100
10 / 100
80 / 100
15 / 100

Polishability

65 / 100
60 / 100
45 / 100
60 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

205 MJ/kg88,134 BTU/lb
205 MJ/kg88,134 BTU/lb
200 MJ/kg85,985 BTU/lb
205 MJ/kg88,134 BTU/lb

Embodied Carbon (primary production)

12.5 kg CO₂/kg
12.5 kg CO₂/kg
13 kg CO₂/kg
12.5 kg CO₂/kg

Embodied Water

1,150 L/kg138 gal/lb
1,200 L/kg144 gal/lb
1,200 L/kg144 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

12%
15%
20%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

174 kN·m/kg
204 kN·m/kg
20 kN·m/kg
129 kN·m/kg

Specific Stiffness (E / density)

25.3 MN·m/kg
25.5 MN·m/kg
25.4 MN·m/kg
25.2 MN·m/kg

Modulus of Resilience

1,248 kJ/m³
1,764 kJ/m³
3 kJ/m³
709 kJ/m³

Thermal Diffusivity

67.1 mm²/s
48.2 mm²/s
92.7 mm²/s
61.7 mm²/s

Thermal Shock Resistance Index

50
44
8
33

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale7072700370757475

Manufacturing and finishing

Capability7475707570727003
CNC machiningYesYesYes
Default conditionT6
Relative cost$$$ Premium$$$ Premium$ Budget$$ Standard
Min. machined wall0.5 mm0.8 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
DLCYesYesYes

Both are offered for Sheet metal. They share 15 finishes: Anodizing Type II, Cerakote, Chem Film (Alodine), E-Coating, Electroless Nickel (EN), Electropolishing, Epoxy Coating, Gold Plating, Hard Anodize Type III w/ PTFE, Hard Anodizing Type III, Nickel Plating, PTFE Coating and 3 more.