FabDigit

3105 vs 3003 and 2 more: properties

3105300330043005

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

69 GPa10 Msi
68.9 GPa10 Msi
69 GPa10 Msi
69 GPa10 Msi

Shear Modulus

26 GPa3.8 Msi
25 GPa3.6 Msi
26 GPa3.8 Msi
26 GPa3.8 Msi

Bulk Modulus

69 GPa10 Msi
69 GPa10 Msi
72 GPa10.4 Msi
70 GPa10.2 Msi

Tensile Strength (Ultimate)

180 MPa26.1 ksi
150 MPa21.8 ksi
240 MPa34.8 ksi
175 MPa25.4 ksi

Yield Strength (0.2% offset)

160 MPa23.2 ksi
145 MPa21 ksi
200 MPa29 ksi
155 MPa22.5 ksi

Elongation at Break

8%
10%
12%
5%

Shear Strength

110 MPa16 ksi
96 MPa13.9 ksi
125 MPa18.1 ksi
105 MPa15.2 ksi

Fatigue Strength (Endurance Limit)

62 MPa9 ksi
62 MPa9 ksi
105 MPa15.2 ksi
65 MPa9.4 ksi

Hardness, Brinell

48 HB
40 HB
63 HB
48 HB

Compressive Strength

205 MPa29.7 ksi

Same in both: Poisson's Ratio 0.33

Physical

Density and transition temperatures.

Density

2.72 g/cm³0.1 lb/in³
2.73 g/cm³0.1 lb/in³
2.72 g/cm³0.1 lb/in³
2.73 g/cm³0.1 lb/in³

Melting Point (Solidus)

635°C1,175 °F
643°C1,189 °F
629°C1,164 °F
630°C1,166 °F

Liquidus Temperature

655°C1,211 °F
654°C1,209 °F
654°C1,209 °F
655°C1,211 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

172 W/m·K99.4 BTU/hr·ft·°F
159 W/m·K91.9 BTU/hr·ft·°F
162 W/m·K93.6 BTU/hr·ft·°F
163 W/m·K94.2 BTU/hr·ft·°F

Specific Heat Capacity

897 J/kg·K0.21 BTU/lb·°F
893 J/kg·K0.21 BTU/lb·°F
893 J/kg·K0.21 BTU/lb·°F
893 J/kg·K0.21 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

23.6 µm/m·K13.1 µin/in·°F
23.2 µm/m·K12.9 µin/in·°F
23.2 µm/m·K12.9 µin/in·°F
23.8 µm/m·K13.2 µin/in·°F

Latent Heat of Fusion

393 J/g169 BTU/lb
390 J/g168 BTU/lb
393 J/g169 BTU/lb
397 J/g171 BTU/lb

Max Service Temperature (continuous)

150°C302 °F
150°C302 °F
150°C302 °F
120°C248 °F

Min Service Temperature

-196°C-321 °F
-196°C-321 °F
-196°C-321 °F
-200°C-328 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

41 % IACS
41 % IACS
42 % IACS
41 % IACS

Electrical Resistivity

4.2×10⁻⁸ Ω·m1.65 µΩ·in
4.2×10⁻⁸ Ω·m1.65 µΩ·in
4.1×10⁻⁸ Ω·m1.61 µΩ·in
4.2×10⁻⁸ Ω·m1.65 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.83 V
-0.83 V
-0.84 V
-0.84 V

Same in both: Corrosion Resistance 68 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

42 / 100
45 / 100
50 / 100
35 / 100

Machinability Rating (AISI 1212 = 100 %)

35%
90%
30%

Weldability

85 / 100
90 / 100
88 / 100
85 / 100

Formability (cold)

70 / 100
70 / 100
65 / 100
70 / 100

Brazeability / Solderability

60 / 100
90 / 100
45 / 100
55 / 100

Polishability

45 / 100
45 / 100
55 / 100
45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

200 MJ/kg85,985 BTU/lb
205 MJ/kg88,134 BTU/lb
200 MJ/kg85,985 BTU/lb
200 MJ/kg85,985 BTU/lb

Embodied Carbon (primary production)

12 kg CO₂/kg
12.5 kg CO₂/kg
12.5 kg CO₂/kg
12.5 kg CO₂/kg

Embodied Water

1,200 L/kg144 gal/lb
1,100 L/kg132 gal/lb
1,200 L/kg144 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

40%
35%
55%
35%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

66 kN·m/kg
55 kN·m/kg
88 kN·m/kg
64 kN·m/kg

Specific Stiffness (E / density)

25.4 MN·m/kg
25.2 MN·m/kg
25.4 MN·m/kg
25.3 MN·m/kg

Modulus of Resilience

186 kJ/m³
153 kJ/m³
290 kJ/m³
174 kJ/m³

Thermal Diffusivity

70.5 mm²/s
65.2 mm²/s
66.7 mm²/s
66.9 mm²/s

Thermal Shock Resistance Index

19
15
24
17

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale3003300430053105

Manufacturing and finishing

Capability3105300330043005
CNC machiningYes
Default condition
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.5 mm
Best machined surfaceRa 0.8 µm
DLCYes

Both are offered for Sheet metal. They share 15 finishes: Anodizing Type II, Cerakote, Chem Film (Alodine), E-Coating, Electroless Nickel (EN), Electropolishing, Epoxy Coating, Gold Plating, Hard Anodize Type III w/ PTFE, Hard Anodizing Type III, Nickel Plating, PTFE Coating and 3 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 3105 and 3003 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.