FabDigitFabDigit

Titanium Grade C-9-F vs Grade C-9-SR

Titanium · Grade C-9 temper comparison

Grade C-9-F and Grade C-9-SR are two conditions of the same titanium grade, Grade C-9: F (as fabricated) versus SR (stress relieved). The chemistry is identical, so every difference below comes from the condition. Both yield at about 520 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (as fabricated versus stress relieved). Grade C-9-SR is the more ductile: elongation 9% versus 8% for Grade C-9-F.

Grade C-9-SRChoose it when the part is bent, formed or impact-loaded.

Grade C-9-F vs Grade C-9-SR: properties

Grade C-9-FGrade C-9-SR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

630 MPa91.4 ksi
640 MPa92.8 ksi

Yield Strength (0.2% offset)

520 MPa75.4 ksi
530 MPa76.9 ksi

Elongation at Break

8%
9%

Reduction in Area

15%
18%

Compressive Strength

690 MPa100 ksi
670 MPa97.2 ksi

Shear Strength

430 MPa62.4 ksi
420 MPa60.9 ksi

Fatigue Strength (Endurance Limit)

240 MPa34.8 ksi
260 MPa37.7 ksi

Fracture Toughness (K_IC)

65 MPa·√m59.2 ksi·√in
72 MPa·√m65.5 ksi·√in

Charpy V-Notch Impact (RT)

16 J11.8 ft·lbf
22 J16.2 ft·lbf

Hardness, Brinell

250 HB
255 HB

Hardness, Rockwell C

23 HRC
24 HRC

Hardness, Vickers

262 HV
267 HV

Same in both: Elastic (Young's) Modulus 100 GPa14.5 Msi · Shear Modulus 40 GPa5.8 Msi · Bulk Modulus 95 GPa13.8 Msi · Poisson's Ratio 0.32

Physical

Density and transition temperatures.

Same in both: Density 4.48 g/cm³0.16 lb/in³ · Melting Point (Solidus) 1,620°C2,948 °F · Liquidus Temperature 1,700°C3,092 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 7.6 W/m·K4.4 BTU/hr·ft·°F · Specific Heat Capacity 544 J/kg·K0.13 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 9.4 µm/m·K5.2 µin/in·°F · Latent Heat of Fusion 365 J/g157 BTU/lb · Max Service Temperature (continuous) 300°C572 °F · Min Service Temperature -250°C-418 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 1.4 % IACS · Electrical Resistivity 1.26×10⁻⁶ Ω·m49.6 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.1 V · Corrosion Resistance 90 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

25 / 100
26 / 100

Machinability Rating (AISI 1212 = 100 %)

22%
23%

Formability (cold)

25 / 100
27 / 100

Same in both: Weldability 80 / 100 · Castability 60 / 100 · Brazeability / Solderability 40 / 100 · Polishability 70 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 680 MJ/kg292,348 BTU/lb · Embodied Carbon (primary production) 45 kg CO₂/kg · Embodied Water 500 L/kg59.9 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every titanium grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

3005007001,0004.555.5Density (g/cm³)Yield strength (MPa) — log scaleGrade C-9

Grade C-9-F vs Grade C-9-SR — frequently asked

What is the difference between Grade C-9-F and Grade C-9-SR?

Grade C-9-F and Grade C-9-SR are two conditions of the same titanium grade, Grade C-9: F (as fabricated) versus SR (stress relieved). The chemistry is identical, so every difference below comes from the condition. Both yield at about 520 MPa — the mechanical properties are the same, and the difference is in how the stock is processed and what it is certified to (as fabricated versus stress relieved).

Which condition does FabDigit quote by default, F or SR?

ANNEAL is the default Grade C-9 condition in the FabDigit quote flow (neither F nor SR). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose Grade C-9-F over Grade C-9-SR?

Pick Grade C-9-SR when the part is bent, formed or impact-loaded.

Ready to make it?

Upload a CAD file and FabDigit prices the part in Grade C-9-F and Grade C-9-SR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.