FabDigitFabDigit

Steel X52-N vs X52-Q

Steel · X52 temper comparison

X52-N and X52-Q are two conditions of the same steel grade, X52: N (normalized) versus Q (L360Q / X52Q). The chemistry is identical, so every difference below comes from the condition. X52-Q is the stronger of the two: yield strength 430 MPa (62.4 ksi) against 405 MPa (58.7 ksi) for X52-N, about 6% more. X52-Q is harder — 175 HB against 160 HB for X52-N — which matters for wear surfaces and threads.

X52-QChoose it when strength drives the design, or when surface hardness matters.

X52-N vs X52-Q: properties

X52-NX52-Q

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

525 MPa76.1 ksi
545 MPa79 ksi

Yield Strength (0.2% offset)

405 MPa58.7 ksi
430 MPa62.4 ksi

Elongation at Break

29%
28%

Reduction in Area

65%
68%

Compressive Strength

405 MPa58.7 ksi
430 MPa62.4 ksi

Shear Strength

325 MPa47.1 ksi
340 MPa49.3 ksi

Fatigue Strength (Endurance Limit)

235 MPa34.1 ksi
255 MPa37 ksi

Fracture Toughness (K_IC)

160 MPa·√m146 ksi·√in
180 MPa·√m164 ksi·√in

Charpy V-Notch Impact (RT)

130 J95.9 ft·lbf
180 J133 ft·lbf

Hardness, Brinell

160 HB
175 HB

Hardness, Rockwell B

84 HRB
88 HRB

Hardness, Vickers

168 HV
185 HV

Same in both: Elastic (Young's) Modulus 207 GPa30 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,460°C2,660 °F · Liquidus Temperature 1,510°C2,750 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

48 W/m·K27.7 BTU/hr·ft·°F
45 W/m·K26 BTU/hr·ft·°F

Min Service Temperature

-45°C-49 °F
-50°C-58 °F

Same in both: Specific Heat Capacity 480 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Max Service Temperature (continuous) 350°C662 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

10 % IACS
9.5 % IACS

Electrical Resistivity

1.7×10⁻⁷ Ω·m6.69 µΩ·in
1.8×10⁻⁷ Ω·m7.09 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.65 V · Corrosion Resistance 12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

62 / 100
58 / 100

Machinability Rating (AISI 1212 = 100 %)

66%
62%

Formability (cold)

78 / 100
76 / 100

Same in both: Weldability 88 / 100 · Brazeability / Solderability 55 / 100 · Polishability 45 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 2.1 kg CO₂/kg · Embodied Water 40 L/kg4.8 gal/lb · Typical Recycled Content 20%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleX52

X52-N vs X52-Q — frequently asked

Is X52-Q stronger than X52-N?

Yes. X52-Q has a typical yield strength of 430 MPa (62.4 ksi) against 405 MPa (58.7 ksi) for X52-N — about 6% more. Tensile strength is 545 MPa (79 ksi) vs 525 MPa (76.1 ksi).

Which condition does FabDigit quote by default, N or Q?

M is the default X52 condition in the FabDigit quote flow (neither N nor Q). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose X52-N over X52-Q?

Pick X52-Q when strength drives the design, or when surface hardness matters.

Ready to make it?

Upload a CAD file and FabDigit prices the part in X52-N and X52-Q side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.