SUM22-CD and SUM22-HR are two conditions of the same steel grade, SUM22: CD (cold drawn) versus HR (hot rolled). The chemistry is identical, so every difference below comes from the condition. SUM22-CD is the stronger of the two: yield strength 415 MPa (60.2 ksi) against 250 MPa (36.3 ksi) for SUM22-HR, about 66% more; tensile strength follows at 540 MPa (78.3 ksi) vs 415 MPa (60.2 ksi). In exchange, SUM22-HR is the more ductile: elongation 25% versus 10% for SUM22-CD, and SUM22-CD is harder (163 HB vs 121 HB).

SUM22-CDChoose it when strength drives the design.

SUM22-HRChoose it when the part is bent, formed or impact-loaded.

SUM22-CD vs SUM22-HR: properties

SUM22-CDSUM22-HR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

540 MPa78.3 ksi
415 MPa60.2 ksi

Yield Strength (0.2% offset)

415 MPa60.2 ksi
250 MPa36.3 ksi

Elongation at Break

10%
25%

Reduction in Area

35%
45%

Fatigue Strength (Endurance Limit)

240 MPa34.8 ksi
190 MPa27.6 ksi

Charpy V-Notch Impact (RT)

25 J18.4 ft·lbf
35 J25.8 ft·lbf

Hardness, Brinell

163 HB
121 HB

Hardness, Rockwell B

84 HRB
67 HRB

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29 · Shear Strength 330 MPa47.9 ksi

Physical

Density and transition temperatures.

Same in both: Density 7.87 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,425°C2,597 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 51 W/m·K29.5 BTU/hr·ft·°F · Specific Heat Capacity 480 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 11.9 µm/m·K6.6 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Max Service Temperature (continuous) 350°C662 °F · Min Service Temperature -20°C-4 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 10 % IACS · Electrical Resistivity 1.7×10⁻⁷ Ω·m6.69 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 8 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

92 / 100
88 / 100

Machinability Rating (AISI 1212 = 100 %)

136%
125%

Formability (cold)

45 / 100
55 / 100

Same in both: Weldability 25 / 100 · Brazeability / Solderability 60 / 100 · Polishability 45 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 1.9 kg CO₂/kg · Embodied Water 45 L/kg5.4 gal/lb · Typical Recycled Content 35%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSUM22

SUM22-CD vs SUM22-HR — frequently asked

Is SUM22-CD stronger than SUM22-HR?

Yes. SUM22-CD has a typical yield strength of 415 MPa (60.2 ksi) against 250 MPa (36.3 ksi) for SUM22-HR — about 66% more. Tensile strength is 540 MPa (78.3 ksi) vs 415 MPa (60.2 ksi).

Which condition does FabDigit quote by default, CD or HR?

CD is the default SUM22 condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose SUM22-CD over SUM22-HR?

Pick SUM22-CD when strength drives the design. Pick SUM22-HR when the part is bent, formed or impact-loaded.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SUM22-CD and SUM22-HR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.