FabDigitFabDigit

Steel S960Q-QT vs S960Q-SR

Steel · S960Q temper comparison

S960Q-QT and S960Q-SR are two conditions of the same steel grade, S960Q: QT (quenched and tempered) versus SR (stress relieved). The chemistry is identical, so every difference below comes from the condition. S960Q-QT is the stronger of the two: yield strength 1,000 MPa (145 ksi) against 950 MPa (138 ksi) for S960Q-SR, about 5% more. S960Q-QT is harder — 33 HRC against 31 HRC for S960Q-SR — which matters for wear surfaces and threads.

S960Q-QTChoose it when strength drives the design, or when surface hardness matters.

S960Q-QT vs S960Q-SR: properties

S960Q-QTS960Q-SR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

1,050 MPa152 ksi
1,010 MPa146 ksi

Yield Strength (0.2% offset)

1,000 MPa145 ksi
950 MPa138 ksi

Elongation at Break

13%
14%

Reduction in Area

55%
57%

Compressive Strength

990 MPa144 ksi
950 MPa138 ksi

Shear Strength

630 MPa91.4 ksi
605 MPa87.7 ksi

Fatigue Strength (Endurance Limit)

480 MPa69.6 ksi
470 MPa68.2 ksi

Fracture Toughness (K_IC)

90 MPa·√m81.9 ksi·√in
95 MPa·√m86.5 ksi·√in

Charpy V-Notch Impact (RT)

70 J51.6 ft·lbf
75 J55.3 ft·lbf

Hardness, Brinell

320 HB
305 HB

Hardness, Rockwell C

33 HRC
31 HRC

Hardness, Vickers

335 HV
320 HV

Same in both: Elastic (Young's) Modulus 210 GPa30.5 Msi · Shear Modulus 81 GPa11.7 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.3

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 32 W/m·K18.5 BTU/hr·ft·°F · Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12 µm/m·K6.7 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Max Service Temperature (continuous) 250°C482 °F · Min Service Temperature -20°C-4 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 7.5 % IACS · Electrical Resistivity 2.3×10⁻⁷ Ω·m9.06 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.6 V · Corrosion Resistance 13 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

33 / 100
36 / 100

Machinability Rating (AISI 1212 = 100 %)

40%
43%

Weldability

55 / 100
58 / 100

Formability (cold)

38 / 100
40 / 100

Same in both: Brazeability / Solderability 40 / 100 · Polishability 50 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 32 MJ/kg13,758 BTU/lb · Embodied Carbon (primary production) 2.5 kg CO₂/kg · Embodied Water 55 L/kg6.6 gal/lb · Typical Recycled Content 25%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleS960Q

S960Q-QT vs S960Q-SR — frequently asked

Is S960Q-QT stronger than S960Q-SR?

Yes. S960Q-QT has a typical yield strength of 1,000 MPa (145 ksi) against 950 MPa (138 ksi) for S960Q-SR — about 5% more. Tensile strength is 1,050 MPa (152 ksi) vs 1,010 MPa (146 ksi).

Which condition does FabDigit quote by default, QT or SR?

QT is the default S960Q condition in the FabDigit quote flow. The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose S960Q-QT over S960Q-SR?

Pick S960Q-QT when strength drives the design, or when surface hardness matters.

Ready to make it?

Upload a CAD file and FabDigit prices the part in S960Q-QT and S960Q-SR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.