FabDigitFabDigit

Steel A516 Gr 60 Annealed vs A516 Gr 60 Normalized

Steel · A516 Gr 60 temper comparison

A516 Gr 60 Annealed and A516 Gr 60 Normalized are two conditions of the same steel grade, A516 Gr 60: Annealed versus Normalized. The chemistry is identical, so every difference below comes from the condition. A516 Gr 60 Normalized is the stronger of the two: yield strength 285 MPa (41.3 ksi) against 250 MPa (36.3 ksi) for A516 Gr 60 Annealed, about 14% more; tensile strength follows at 470 MPa (68.2 ksi) vs 440 MPa (63.8 ksi). A516 Gr 60 Normalized is harder — 135 HB against 122 HB for A516 Gr 60 Annealed — which matters for wear surfaces and threads.

A516 Gr 60 NormalizedChoose it when strength drives the design, or when surface hardness matters.

A516 Gr 60 Annealed vs A516 Gr 60 Normalized: properties

A516 Gr 60 AnnealedA516 Gr 60 Normalized

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

440 MPa63.8 ksi
470 MPa68.2 ksi

Yield Strength (0.2% offset)

250 MPa36.3 ksi
285 MPa41.3 ksi

Elongation at Break

30%
29%

Reduction in Area

58%
60%

Fatigue Strength (Endurance Limit)

190 MPa27.6 ksi
210 MPa30.5 ksi

Fracture Toughness (K_IC)

130 MPa·√m118 ksi·√in
150 MPa·√m137 ksi·√in

Charpy V-Notch Impact (RT)

50 J36.9 ft·lbf
85 J62.7 ft·lbf

Hardness, Brinell

122 HB
135 HB

Same in both: Elastic (Young's) Modulus 203 GPa29.4 Msi · Shear Modulus 79 GPa11.5 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29 · Compressive Strength 265 MPa38.4 ksi · Shear Strength 290 MPa42.1 ksi · Hardness, Rockwell B 72 HRB · Hardness, Vickers 137 HV

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,490°C2,714 °F · Liquidus Temperature 1,520°C2,768 °F

Thermal

How each material carries heat and how hot it can run.

Min Service Temperature

-29°C-20 °F
-46°C-51 °F

Same in both: Thermal Conductivity 52 W/m·K30 BTU/hr·ft·°F · Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 11.9 µm/m·K6.6 µin/in·°F · Latent Heat of Fusion 270 J/g116 BTU/lb · Max Service Temperature (continuous) 425°C797 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 10 % IACS · Electrical Resistivity 1.7×10⁻⁷ Ω·m6.69 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.65 V · Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability Rating (AISI 1212 = 100 %)

72%
68%

Weldability

92 / 100
90 / 100

Formability (cold)

82 / 100
76 / 100

Same in both: Machinability 65 / 100 · Brazeability / Solderability 60 / 100 · Polishability 40 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 1.9 kg CO₂/kg · Embodied Water 40 L/kg4.8 gal/lb · Typical Recycled Content 25%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleA516 Gr 60

A516 Gr 60 Annealed vs A516 Gr 60 Normalized — frequently asked

Is A516 Gr 60 Normalized stronger than A516 Gr 60 Annealed?

Yes. A516 Gr 60 Normalized has a typical yield strength of 285 MPa (41.3 ksi) against 250 MPa (36.3 ksi) for A516 Gr 60 Annealed — about 14% more. Tensile strength is 470 MPa (68.2 ksi) vs 440 MPa (63.8 ksi).

Which condition does FabDigit quote by default, Annealed or Normalized?

HR is the default A516 Gr 60 condition in the FabDigit quote flow (neither Annealed nor Normalized). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

When should I choose A516 Gr 60 Annealed over A516 Gr 60 Normalized?

Pick A516 Gr 60 Normalized when strength drives the design, or when surface hardness matters.

Ready to make it?

Upload a CAD file and FabDigit prices the part in A516 Gr 60 Annealed and A516 Gr 60 Normalized side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.