FabDigitFabDigit

Steel 50B44-CD vs 50B44-N

Steel · 50B44 temper comparison

50B44-CD and 50B44-N are two conditions of the same steel grade, 50B44: CD (cold drawn) versus N (normalized). The chemistry is identical, so every difference below comes from the condition. 50B44-CD is the stronger of the two: yield strength 640 MPa (92.8 ksi) against 520 MPa (75.4 ksi) for 50B44-N, about 23% more. In exchange, 50B44-N is the more ductile: elongation 20% versus 12% for 50B44-CD, and 50B44-N is harder (248 HB vs 217 HB). 50B44-N runs hotter in service (400°C vs 300°C continuous).

50B44-CDChoose it when strength drives the design.

50B44-NChoose it when the part is bent, formed or impact-loaded, or when the part sees heat.

50B44-CD vs 50B44-N: properties

50B44-CD50B44-N

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

760 MPa110 ksi
840 MPa122 ksi

Yield Strength (0.2% offset)

640 MPa92.8 ksi
520 MPa75.4 ksi

Elongation at Break

12%
20%

Reduction in Area

38%
50%

Shear Strength

460 MPa66.7 ksi
420 MPa60.9 ksi

Fatigue Strength (Endurance Limit)

340 MPa49.3 ksi
380 MPa55.1 ksi

Charpy V-Notch Impact (RT)

18 J13.3 ft·lbf
24 J17.7 ft·lbf

Hardness, Brinell

217 HB
248 HB

Hardness, Rockwell B

96 HRB
90 HRB

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,490°C2,714 °F

Thermal

How each material carries heat and how hot it can run.

Max Service Temperature (continuous)

300°C572 °F
400°C752 °F

Same in both: Thermal Conductivity 44 W/m·K25.4 BTU/hr·ft·°F · Specific Heat Capacity 475 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12.2 µm/m·K6.8 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Min Service Temperature -30°C-22 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 8 % IACS · Electrical Resistivity 2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

60 / 100
51 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
55%

Weldability

25 / 100
30 / 100

Formability (cold)

25 / 100
45 / 100

Same in both: Brazeability / Solderability 55 / 100 · Polishability 55 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 1.9 kg CO₂/kg · Embodied Water 50 L/kg6 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale50B44

50B44-CD vs 50B44-N — frequently asked

Is 50B44-CD stronger than 50B44-N?

Yes. 50B44-CD has a typical yield strength of 640 MPa (92.8 ksi) against 520 MPa (75.4 ksi) for 50B44-N — about 23% more. Tensile strength is 760 MPa (110 ksi) vs 840 MPa (122 ksi).

Which condition does FabDigit quote by default, CD or N?

A is the default 50B44 condition in the FabDigit quote flow (neither CD nor N). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 50B44-CD or 50B44-N?

50B44-CD. Its machinability rates good (60/100) against fair (51/100) for 50B44-N; for welding the order is 50B44-N first (poor, 30/100) then 50B44-CD (poor, 25/100).

Ready to make it?

Upload a CAD file and FabDigit prices the part in 50B44-CD and 50B44-N side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.