FabDigitFabDigit

Steel 4047-CD vs 4047-N

Steel · 4047 temper comparison

4047-CD and 4047-N are two conditions of the same steel grade, 4047: CD (cold drawn) versus N (normalized). The chemistry is identical, so every difference below comes from the condition. 4047-CD is the stronger of the two: yield strength 650 MPa (94.3 ksi) against 510 MPa (74 ksi) for 4047-N, about 27% more. In exchange, 4047-N is the more ductile: elongation 19% versus 12% for 4047-CD. 4047-N runs hotter in service (425°C vs 350°C continuous). On the shop floor, 4047-CD machines more easily (good vs fair).

4047-CDChoose it when strength drives the design, or when the part is machined in volume.

4047-NChoose it when the part is bent, formed or impact-loaded, or when the part sees heat.

4047-CD vs 4047-N: properties

4047-CD4047-N

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

760 MPa110 ksi
810 MPa117 ksi

Yield Strength (0.2% offset)

650 MPa94.3 ksi
510 MPa74 ksi

Elongation at Break

12%
19%

Reduction in Area

35%
45%

Compressive Strength

650 MPa94.3 ksi
510 MPa74 ksi

Shear Strength

460 MPa66.7 ksi
490 MPa71.1 ksi

Fatigue Strength (Endurance Limit)

340 MPa49.3 ksi
380 MPa55.1 ksi

Fracture Toughness (K_IC)

50 MPa·√m45.5 ksi·√in
55 MPa·√m50.1 ksi·√in

Charpy V-Notch Impact (RT)

12 J8.9 ft·lbf
20 J14.8 ft·lbf

Hardness, Brinell

225 HB
235 HB

Hardness, Rockwell B

97 HRB
99 HRB

Hardness, Vickers

236 HV
247 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,490°C2,714 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

43 W/m·K24.8 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Max Service Temperature (continuous)

350°C662 °F
425°C797 °F

Same in both: Specific Heat Capacity 475 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 12.2 µm/m·K6.8 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Min Service Temperature -30°C-22 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 7.8 % IACS · Electrical Resistivity 2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 11 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

60 / 100
49 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
52%

Formability (cold)

22 / 100
24 / 100

Same in both: Weldability 26 / 100 · Brazeability / Solderability 55 / 100 · Polishability 60 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 29 MJ/kg12,468 BTU/lb · Embodied Carbon (primary production) 2 kg CO₂/kg · Embodied Water 50 L/kg6 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale4047

4047-CD vs 4047-N — frequently asked

Is 4047-CD stronger than 4047-N?

Yes. 4047-CD has a typical yield strength of 650 MPa (94.3 ksi) against 510 MPa (74 ksi) for 4047-N — about 27% more. Tensile strength is 760 MPa (110 ksi) vs 810 MPa (117 ksi).

Which condition does FabDigit quote by default, CD or N?

A is the default 4047 condition in the FabDigit quote flow (neither CD nor N). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 4047-CD or 4047-N?

4047-CD. Its machinability rates good (60/100) against fair (49/100) for 4047-N.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 4047-CD and 4047-N side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.