FabDigitFabDigit

Steel 20MC5-CD vs 20MC5 +S

Steel · 20MC5 temper comparison

20MC5-CD and 20MC5 +S are two conditions of the same steel grade, 20MC5: CD (cold drawn) versus +S (treated for cold shearing / cold heading). The chemistry is identical, so every difference below comes from the condition. 20MC5-CD is the stronger of the two: yield strength 600 MPa (87 ksi) against 360 MPa (52.2 ksi) for 20MC5 +S, about 67% more; tensile strength follows at 750 MPa (109 ksi) vs 560 MPa (81.2 ksi). In exchange, 20MC5 +S is the more ductile: elongation 25% versus 11% for 20MC5-CD, and 20MC5-CD is harder (230 HB vs 165 HB).

20MC5-CDChoose it when strength drives the design.

20MC5 +SChoose it when the part is bent, formed or impact-loaded.

20MC5-CD vs 20MC5 +S: properties

20MC5-CD20MC5 +S

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

750 MPa109 ksi
560 MPa81.2 ksi

Yield Strength (0.2% offset)

600 MPa87 ksi
360 MPa52.2 ksi

Elongation at Break

11%
25%

Reduction in Area

40%
58%

Shear Strength

450 MPa65.3 ksi
340 MPa49.3 ksi

Fatigue Strength (Endurance Limit)

340 MPa49.3 ksi
255 MPa37 ksi

Fracture Toughness (K_IC)

65 MPa·√m59.2 ksi·√in
85 MPa·√m77.4 ksi·√in

Charpy V-Notch Impact (RT)

30 J22.1 ft·lbf
85 J62.7 ft·lbf

Hardness, Brinell

230 HB
165 HB

Hardness, Rockwell B

98 HRB
85 HRB

Same in both: Elastic (Young's) Modulus 210 GPa30.5 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Same in both: Thermal Conductivity 44 W/m·K25.4 BTU/hr·ft·°F · Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 11.7 µm/m·K6.5 µin/in·°F · Latent Heat of Fusion 270 J/g116 BTU/lb · Max Service Temperature (continuous) 200°C392 °F · Min Service Temperature -40°C-40 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Resistivity 2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

60 / 100
52 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
57%

Weldability

35 / 100
42 / 100

Formability (cold)

40 / 100
70 / 100

Same in both: Castability 25 / 100 · Brazeability / Solderability 60 / 100 · Polishability 55 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 29 MJ/kg12,468 BTU/lb · Embodied Carbon (primary production) 2.1 kg CO₂/kg · Embodied Water 45 L/kg5.4 gal/lb · Typical Recycled Content 30%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale20MC5

20MC5-CD vs 20MC5 +S — frequently asked

Is 20MC5-CD stronger than 20MC5 +S?

Yes. 20MC5-CD has a typical yield strength of 600 MPa (87 ksi) against 360 MPa (52.2 ksi) for 20MC5 +S — about 67% more. Tensile strength is 750 MPa (109 ksi) vs 560 MPa (81.2 ksi).

Which condition does FabDigit quote by default, CD or +S?

+A is the default 20MC5 condition in the FabDigit quote flow (neither CD nor +S). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 20MC5-CD or 20MC5 +S?

20MC5-CD. Its machinability rates good (60/100) against fair (52/100) for 20MC5 +S; for welding the order is 20MC5 +S first (fair, 42/100) then 20MC5-CD (fair, 35/100).

Ready to make it?

Upload a CAD file and FabDigit prices the part in 20MC5-CD and 20MC5 +S side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.