FabDigitFabDigit

Steel 15B62-CD vs 15B62-N

Steel · 15B62 temper comparison

15B62-CD and 15B62-N are two conditions of the same steel grade, 15B62: CD (cold drawn) versus N (normalized). The chemistry is identical, so every difference below comes from the condition. 15B62-CD is the stronger of the two: yield strength 730 MPa (106 ksi) against 570 MPa (82.7 ksi) for 15B62-N, about 28% more. 15B62-N is harder — 290 HB against 250 HB for 15B62-CD — which matters for wear surfaces and threads. 15B62-N runs hotter in service (300°C vs 230°C continuous).

15B62-CDChoose it when strength drives the design.

15B62-NChoose it when surface hardness matters, or when the part sees heat.

15B62-CD vs 15B62-N: properties

15B62-CD15B62-N

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

860 MPa125 ksi
1,000 MPa145 ksi

Yield Strength (0.2% offset)

730 MPa106 ksi
570 MPa82.7 ksi

Elongation at Break

10%
11%

Reduction in Area

30%
28%

Shear Strength

540 MPa78.3 ksi
640 MPa92.8 ksi

Fatigue Strength (Endurance Limit)

380 MPa55.1 ksi
440 MPa63.8 ksi

Fracture Toughness (K_IC)

58 MPa·√m52.8 ksi·√in
55 MPa·√m50.1 ksi·√in

Charpy V-Notch Impact (RT)

11 J8.1 ft·lbf
14 J10.3 ft·lbf

Hardness, Brinell

250 HB
290 HB

Hardness, Rockwell B

100 HRB
103 HRB

Hardness, Vickers

263 HV
305 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.85 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,480°C2,696 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

45 W/m·K26 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F

Max Service Temperature (continuous)

230°C446 °F
300°C572 °F

Same in both: Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 11.5 µm/m·K6.4 µin/in·°F · Latent Heat of Fusion 250 J/g107 BTU/lb · Min Service Temperature -30°C-22 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

2.1×10⁻⁷ Ω·m8.27 µΩ·in
2.15×10⁻⁷ Ω·m8.46 µΩ·in

Same in both: Electrical Conductivity 8 % IACS

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.61 V · Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

46 / 100
38 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
50%

Formability (cold)

22 / 100
18 / 100

Same in both: Weldability 18 / 100 · Brazeability / Solderability 40 / 100 · Polishability 55 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 1.9 kg CO₂/kg · Embodied Water 45 L/kg5.4 gal/lb · Typical Recycled Content 35%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale15B62

15B62-CD vs 15B62-N — frequently asked

Is 15B62-CD stronger than 15B62-N?

Yes. 15B62-CD has a typical yield strength of 730 MPa (106 ksi) against 570 MPa (82.7 ksi) for 15B62-N — about 28% more. Tensile strength is 860 MPa (125 ksi) vs 1,000 MPa (145 ksi).

Which condition does FabDigit quote by default, CD or N?

HR is the default 15B62 condition in the FabDigit quote flow (neither CD nor N). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 15B62-CD or 15B62-N?

15B62-CD, by a small margin. Both rate fair for machinability — 46/100 against 38/100 for 15B62-N.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 15B62-CD and 15B62-N side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.