Steel · 1213 temper comparison

1213-ANN and 1213 CD-SR are two conditions of the same steel grade, 1213: ANN (annealed) versus CD-SR (cold drawn, stress relieved). The chemistry is identical, so every difference below comes from the condition. 1213 CD-SR is the stronger of the two: yield strength 380 MPa (55.1 ksi) against 225 MPa (32.6 ksi) for 1213-ANN, about 69% more; tensile strength follows at 505 MPa (73.2 ksi) vs 380 MPa (55.1 ksi). In exchange, 1213-ANN is the more ductile: elongation 30% versus 14% for 1213 CD-SR, and 1213 CD-SR is harder (156 HB vs 110 HB). On the shop floor, 1213 CD-SR machines more easily (excellent vs very good).

1213-ANNChoose it when the part is bent, formed or impact-loaded.

1213 CD-SRChoose it when strength drives the design, or when the part is machined in volume.

1213-ANN vs 1213 CD-SR: properties

1213-ANN1213 CD-SR

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

380 MPa55.1 ksi
505 MPa73.2 ksi

Yield Strength (0.2% offset)

225 MPa32.6 ksi
380 MPa55.1 ksi

Elongation at Break

30%
14%

Reduction in Area

50%
40%

Compressive Strength

225 MPa32.6 ksi
380 MPa55.1 ksi

Shear Strength

265 MPa38.4 ksi
345 MPa50 ksi

Fatigue Strength (Endurance Limit)

170 MPa24.7 ksi
215 MPa31.2 ksi

Charpy V-Notch Impact (RT)

38 J28 ft·lbf
28 J20.7 ft·lbf

Hardness, Brinell

110 HB
156 HB

Hardness, Rockwell B

62 HRB
82 HRB

Hardness, Vickers

115 HV
163 HV

Same in both: Elastic (Young's) Modulus 200 GPa29 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 140 GPa20.3 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Same in both: Density 7.87 g/cm³0.28 lb/in³ · Melting Point (Solidus) 1,420°C2,588 °F · Liquidus Temperature 1,500°C2,732 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

52 W/m·K30 BTU/hr·ft·°F
51.9 W/m·K30 BTU/hr·ft·°F

Same in both: Specific Heat Capacity 486 J/kg·K0.12 BTU/lb·°F · Thermal Expansion (CTE, 20–100 °C) 11.9 µm/m·K6.6 µin/in·°F · Latent Heat of Fusion 247 J/g106 BTU/lb · Max Service Temperature (continuous) 400°C752 °F · Min Service Temperature -20°C-4 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

11 % IACS
10.8 % IACS

Electrical Resistivity

1.57×10⁻⁷ Ω·m6.18 µΩ·in
1.6×10⁻⁷ Ω·m6.3 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Same in both: Galvanic Potential (seawater, vs SCE) -0.6 V · Corrosion Resistance 8 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

80 / 100
92 / 100

Machinability Rating (AISI 1212 = 100 %)

110%
136%

Weldability

16 / 100
15 / 100

Formability (cold)

55 / 100
38 / 100

Same in both: Brazeability / Solderability 55 / 100 · Polishability 35 / 100

Sustainability

Primary-production footprint per kilogram.

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb · Embodied Carbon (primary production) 1.9 kg CO₂/kg · Embodied Water 40 L/kg4.8 gal/lb · Typical Recycled Content 35%

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale1213

1213-ANN vs 1213 CD-SR — frequently asked

Is 1213 CD-SR stronger than 1213-ANN?

Yes. 1213 CD-SR has a typical yield strength of 380 MPa (55.1 ksi) against 225 MPa (32.6 ksi) for 1213-ANN — about 69% more. Tensile strength is 505 MPa (73.2 ksi) vs 380 MPa (55.1 ksi).

Which condition does FabDigit quote by default, ANN or CD-SR?

CD is the default 1213 condition in the FabDigit quote flow (neither ANN nor CD-SR). The other condition is available on request or by drawing note — specify it in the material field or the part notes and the quote is priced for it.

Which is easier to machine, 1213-ANN or 1213 CD-SR?

1213 CD-SR. Its machinability rates excellent (92/100) against very good (80/100) for 1213-ANN.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 1213-ANN and 1213 CD-SR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.