FabDigit

W1 vs A2 and 2 more: properties

W1A2A3O1

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
203 GPa29.4 Msi
203 GPa29.4 Msi
205 GPa29.7 Msi

Shear Modulus

80 GPa11.6 Msi
78 GPa11.3 Msi
79 GPa11.5 Msi
79 GPa11.5 Msi

Poisson's Ratio

0.29
0.28
0.29
0.29

Tensile Strength (Ultimate)

760 MPa110 ksi
740 MPa107 ksi
760 MPa110 ksi
690 MPa100 ksi

Yield Strength (0.2% offset)

460 MPa66.7 ksi
470 MPa68.2 ksi
430 MPa62.4 ksi
400 MPa58 ksi

Elongation at Break

22%
22%
20%
25%

Reduction in Area

45%
45%
35%
45%

Compressive Strength

500 MPa72.5 ksi
500 MPa72.5 ksi
900 MPa131 ksi
420 MPa60.9 ksi

Shear Strength

470 MPa68.2 ksi
450 MPa65.3 ksi
460 MPa66.7 ksi
420 MPa60.9 ksi

Fatigue Strength (Endurance Limit)

330 MPa47.9 ksi
330 MPa47.9 ksi
320 MPa46.4 ksi

Charpy V-Notch Impact (RT)

25 J18.4 ft·lbf
30 J22.1 ft·lbf
25 J18.4 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

200 HB
217 HB
217 HB
200 HB

Hardness, Rockwell B

93 HRB
96 HRB
96 HRB
94 HRB

Hardness, Vickers

210 HV
230 HV
228 HV
210 HV

Hardness, Rockwell C

19 HRC

Same in both: Bulk Modulus 160 GPa23.2 Msi

Physical

Density and transition temperatures.

Density

7.83 g/cm³0.28 lb/in³
7.86 g/cm³0.28 lb/in³
7.86 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,425°C2,597 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,400°C2,552 °F

Liquidus Temperature

1,470°C2,678 °F
1,465°C2,669 °F
1,470°C2,678 °F
1,460°C2,660 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

48 W/m·K27.7 BTU/hr·ft·°F
26 W/m·K15 BTU/hr·ft·°F
24 W/m·K13.9 BTU/hr·ft·°F
35 W/m·K20.2 BTU/hr·ft·°F

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
460 J/kg·K0.11 BTU/lb·°F
460 J/kg·K0.11 BTU/lb·°F
460 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.4 µm/m·K6.9 µin/in·°F
10.7 µm/m·K5.9 µin/in·°F
10.7 µm/m·K5.9 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Max Service Temperature (continuous)

300°C572 °F
425°C797 °F
200°C392 °F
400°C752 °F

Min Service Temperature

-20°C-4 °F
-30°C-22 °F
-30°C-22 °F
-30°C-22 °F

Same in both: Latent Heat of Fusion 250 J/g107 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

9.5 % IACS
2.7 % IACS
2.7 % IACS
7 % IACS

Electrical Resistivity

1.8×10⁻⁷ Ω·m7.09 µΩ·in
6.5×10⁻⁷ Ω·m25.6 µΩ·in
6.5×10⁻⁷ Ω·m25.6 µΩ·in
2.5×10⁻⁷ Ω·m9.84 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.6 V
-0.6 V

Corrosion Resistance

8 / 100
20 / 100
16 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
45 / 100
38 / 100
45 / 100

Machinability Rating (AISI 1212 = 100 %)

30%
60%
42%
42%

Weldability

15 / 100
20 / 100
15 / 100
20 / 100

Formability (cold)

35 / 100
35 / 100
20 / 100
35 / 100

Brazeability / Solderability

45 / 100
40 / 100
35 / 100
45 / 100

Polishability

75 / 100
70 / 100
70 / 100
80 / 100

Castability

20 / 100
25 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

32 MJ/kg13,758 BTU/lb
36 MJ/kg15,477 BTU/lb
36 MJ/kg15,477 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
2.6 kg CO₂/kg
2.6 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

55 L/kg6.6 gal/lb
65 L/kg7.8 gal/lb
60 L/kg7.2 gal/lb
55 L/kg6.6 gal/lb

Typical Recycled Content

30%
35%
30%
40%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

97 kN·m/kg
94 kN·m/kg
97 kN·m/kg
88 kN·m/kg

Specific Stiffness (E / density)

26.2 MN·m/kg
25.8 MN·m/kg
25.8 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

516 kJ/m³
544 kJ/m³
455 kJ/m³
390 kJ/m³

Thermal Diffusivity

13 mm²/s
7.2 mm²/s
6.6 mm²/s
9.7 mm²/s

Thermal Shock Resistance Index

14
9
8
10

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleA2A3O1W1

Manufacturing and finishing

CapabilityW1A2A3O1
Default conditionAnnealedAnnealedAnnealed
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$$ High
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in W1 and A2 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.