FabDigit

Steel T10A vs SK5 vs T12A vs T7A

Benchmark · 4 materials

Side-by-side benchmark of 4 steel grades.

T10A vs SK5 and 2 more: properties

T10ASK5T12AT7A

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

207 GPa30 Msi
205 GPa29.7 Msi
210 GPa30.5 Msi
207 GPa30 Msi

Shear Modulus

80 GPa11.6 Msi
80 GPa11.6 Msi
81 GPa11.7 Msi
80 GPa11.6 Msi

Bulk Modulus

160 GPa23.2 Msi
160 GPa23.2 Msi
165 GPa23.9 Msi
160 GPa23.2 Msi

Tensile Strength (Ultimate)

700 MPa102 ksi
710 MPa103 ksi
720 MPa104 ksi
660 MPa95.7 ksi

Yield Strength (0.2% offset)

400 MPa58 ksi
400 MPa58 ksi
420 MPa60.9 ksi
380 MPa55.1 ksi

Elongation at Break

22%
12%
20%
22%

Reduction in Area

45%
20%
40%
40%

Compressive Strength

800 MPa116 ksi
720 MPa104 ksi
430 MPa62.4 ksi
400 MPa58 ksi

Shear Strength

480 MPa69.6 ksi
460 MPa66.7 ksi
450 MPa65.3 ksi
430 MPa62.4 ksi

Fatigue Strength (Endurance Limit)

320 MPa46.4 ksi
320 MPa46.4 ksi
320 MPa46.4 ksi
300 MPa43.5 ksi

Charpy V-Notch Impact (RT)

25 J18.4 ft·lbf
10 J7.4 ft·lbf
12 J8.9 ft·lbf
40 J29.5 ft·lbf

Hardness, Brinell

187 HB
200 HB
200 HB
180 HB

Hardness, Rockwell B

90 HRB
93 HRB
93 HRB
89 HRB

Hardness, Vickers

195 HV
210 HV
210 HV
190 HV

Fracture Toughness (K_IC)

45 MPa·√m41 ksi·√in
50 MPa·√m45.5 ksi·√in

Same in both: Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Density

7.81 g/cm³0.28 lb/in³
7.82 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.83 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,400°C2,552 °F
1,425°C2,597 °F
1,300°C2,372 °F
1,420°C2,588 °F

Liquidus Temperature

1,470°C2,678 °F
1,470°C2,678 °F
1,440°C2,624 °F
1,480°C2,696 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

47 W/m·K27.2 BTU/hr·ft·°F
48 W/m·K27.7 BTU/hr·ft·°F
47 W/m·K27.2 BTU/hr·ft·°F
48 W/m·K27.7 BTU/hr·ft·°F

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

11.5 µm/m·K6.4 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F
11.8 µm/m·K6.6 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F

Max Service Temperature (continuous)

300°C572 °F
350°C662 °F
400°C752 °F
300°C572 °F

Same in both: Latent Heat of Fusion 250 J/g107 BTU/lb · Min Service Temperature -20°C-4 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 9.5 % IACS · Electrical Resistivity 1.8×10⁻⁷ Ω·m7.09 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.62 V
-0.61 V

Corrosion Resistance

10 / 100
10 / 100
9 / 100
10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
36 / 100
45 / 100
62 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
40%
45%
65%

Weldability

15 / 100
18 / 100
12 / 100
20 / 100

Formability (cold)

40 / 100
30 / 100
40 / 100
45 / 100

Brazeability / Solderability

50 / 100
45 / 100
50 / 100
55 / 100

Castability

30 / 100
30 / 100

Same in both: Polishability 70 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

30 MJ/kg12,898 BTU/lb
27 MJ/kg11,608 BTU/lb
28 MJ/kg12,038 BTU/lb
26 MJ/kg11,178 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.1 kg CO₂/kg
2.1 kg CO₂/kg
2.1 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb
60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

30%
30%
30%
25%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

90 kN·m/kg
91 kN·m/kg
92 kN·m/kg
84 kN·m/kg

Specific Stiffness (E / density)

26.5 MN·m/kg
26.2 MN·m/kg
26.8 MN·m/kg
26.4 MN·m/kg

Modulus of Resilience

386 kJ/m³
390 kJ/m³
420 kJ/m³
349 kJ/m³

Thermal Diffusivity

12.8 mm²/s
12.9 mm²/s
12.7 mm²/s
13 mm²/s

Thermal Shock Resistance Index

14
14
14
13

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSK5T10AT12AT7A

Manufacturing and finishing

CapabilityT10ASK5T12AT7A
CNC machiningYes
Sheet metalYes
Default conditionHR
Relative cost$ Budget$$ Standard$ Budget$ Budget
Min. machined wall0.8 mm
Best machined surfaceRa 1.6 µm
AlCrNYes
AlTiNYes
Black OxideYes
CVD Al2O3Yes
CVD TiCNYes
CVD TiNYes
CerakoteYes
Chrome PlatingYes
CrNYes
DLCYes
E-CoatingYes
HVOF CoatingYes
Hot-Dip GalvanizingYes
MoS2Yes
Multilayer CVDYes
Nickel PlatingYes
PTFE CoatingYes
PaintingYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in T10A and SK5 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.