FabDigit

T1 vs M42 and 2 more: properties

T1M42T8W6Mo5Cr4V2

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

220 GPa31.9 Msi
222 GPa32.2 Msi
220 GPa31.9 Msi
217 GPa31.5 Msi

Shear Modulus

84 GPa12.2 Msi
86 GPa12.5 Msi
85 GPa12.3 Msi
84 GPa12.2 Msi

Bulk Modulus

165 GPa23.9 Msi
165 GPa23.9 Msi
170 GPa24.7 Msi
165 GPa23.9 Msi

Poisson's Ratio

0.28
0.28
0.29
0.28

Tensile Strength (Ultimate)

860 MPa125 ksi
900 MPa131 ksi
900 MPa131 ksi
850 MPa123 ksi

Yield Strength (0.2% offset)

560 MPa81.2 ksi
620 MPa89.9 ksi
570 MPa82.7 ksi
570 MPa82.7 ksi

Elongation at Break

20%
12%
15%
12%

Reduction in Area

32%
20%
25%
20%

Compressive Strength

1,400 MPa203 ksi
680 MPa98.6 ksi
1,200 MPa174 ksi
1,100 MPa160 ksi

Shear Strength

550 MPa79.8 ksi
545 MPa79 ksi
550 MPa79.8 ksi

Charpy V-Notch Impact (RT)

25 J18.4 ft·lbf
9 J6.6 ft·lbf
25 J18.4 ft·lbf
20 J14.8 ft·lbf

Hardness, Brinell

235 HB
255 HB
240 HB
240 HB

Hardness, Rockwell B

99 HRB
101 HRB
99 HRB
99 HRB

Hardness, Vickers

245 HV
270 HV
250 HV
250 HV

Fatigue Strength (Endurance Limit)

400 MPa58 ksi
380 MPa55.1 ksi

Fracture Toughness (K_IC)

33 MPa·√m30 ksi·√in
45 MPa·√m41 ksi·√in

Hardness, Rockwell C

25 HRC
23 HRC

Physical

Density and transition temperatures.

Density

8.7 g/cm³0.31 lb/in³
7.98 g/cm³0.29 lb/in³
8.6 g/cm³0.31 lb/in³
8.16 g/cm³0.29 lb/in³

Melting Point (Solidus)

1,340°C2,444 °F
1,290°C2,354 °F
1,400°C2,552 °F
1,250°C2,282 °F

Liquidus Temperature

1,440°C2,624 °F
1,420°C2,588 °F
1,460°C2,660 °F
1,430°C2,606 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

21 W/m·K12.1 BTU/hr·ft·°F
22 W/m·K12.7 BTU/hr·ft·°F
22 W/m·K12.7 BTU/hr·ft·°F
24 W/m·K13.9 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

11 µm/m·K6.1 µin/in·°F
10.8 µm/m·K6 µin/in·°F
11.2 µm/m·K6.2 µin/in·°F
10.1 µm/m·K5.6 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
250 J/g107 BTU/lb
260 J/g112 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
400°C752 °F
500°C932 °F

Min Service Temperature

-60°C-76 °F
-60°C-76 °F
-40°C-40 °F
-60°C-76 °F

Same in both: Specific Heat Capacity 420 J/kg·K0.1 BTU/lb·°F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 3.1 % IACS · Electrical Resistivity 5.5×10⁻⁷ Ω·m21.7 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.55 V
-0.6 V

Corrosion Resistance

22 / 100
18 / 100
18 / 100
18 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

35 / 100
38 / 100
35 / 100
40 / 100

Machinability Rating (AISI 1212 = 100 %)

30%
42%
40%
45%

Weldability

15 / 100
20 / 100
15 / 100
18 / 100

Formability (cold)

15 / 100
10 / 100
12 / 100
15 / 100

Castability

25 / 100
20 / 100
30 / 100

Polishability

60 / 100
80 / 100
70 / 100
70 / 100

Same in both: Brazeability / Solderability 55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

52 MJ/kg22,356 BTU/lb
62 MJ/kg26,655 BTU/lb
60 MJ/kg25,795 BTU/lb
55 MJ/kg23,646 BTU/lb

Embodied Carbon (primary production)

3.6 kg CO₂/kg
4.4 kg CO₂/kg
4.2 kg CO₂/kg
3.6 kg CO₂/kg

Typical Recycled Content

45%
30%
35%
40%

Same in both: Embodied Water 90 L/kg10.8 gal/lb

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

99 kN·m/kg
113 kN·m/kg
105 kN·m/kg
104 kN·m/kg

Specific Stiffness (E / density)

25.3 MN·m/kg
27.8 MN·m/kg
25.6 MN·m/kg
26.6 MN·m/kg

Modulus of Resilience

713 kJ/m³
866 kJ/m³
738 kJ/m³
749 kJ/m³

Thermal Diffusivity

5.7 mm²/s
6.6 mm²/s
6.1 mm²/s
7 mm²/s

Thermal Shock Resistance Index

7
8
8
9

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleM42T8T1W6Mo5Cr4V2

Manufacturing and finishing

CapabilityT1M42T8W6Mo5Cr4V2
Default conditionAnnealedAnnealedAnnealedAnnealed
Relative cost$$$ Premium$$$$$ Specialty$$$ Premium$$$ Premium
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in T1 and M42 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.