FabDigit

SPHC vs A283 and 2 more: properties

SPHCA283A656A36

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
200 GPa29 Msi
200 GPa29 Msi
200 GPa29 Msi

Shear Modulus

79 GPa11.5 Msi
79 GPa11.5 Msi
79 GPa11.5 Msi
79.3 GPa11.5 Msi

Tensile Strength (Ultimate)

310 MPa45 ksi
420 MPa60.9 ksi
660 MPa95.7 ksi
450 MPa65.3 ksi

Yield Strength (0.2% offset)

240 MPa34.8 ksi
230 MPa33.4 ksi
580 MPa84.1 ksi
260 MPa37.7 ksi

Elongation at Break

38%
25%
16%
22%

Reduction in Area

60%
45%
50%
50%

Shear Strength

210 MPa30.5 ksi
270 MPa39.2 ksi
420 MPa60.9 ksi
275 MPa39.9 ksi

Fatigue Strength (Endurance Limit)

155 MPa22.5 ksi
190 MPa27.6 ksi
290 MPa42.1 ksi
200 MPa29 ksi

Fracture Toughness (K_IC)

120 MPa·√m109 ksi·√in
90 MPa·√m81.9 ksi·√in
100 MPa·√m91 ksi·√in
100 MPa·√m91 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
27 J19.9 ft·lbf
80 J59 ft·lbf
55 J40.6 ft·lbf

Hardness, Brinell

110 HB
120 HB
215 HB
120 HB

Hardness, Rockwell B

64 HRB
68 HRB
96 HRB
67 HRB

Hardness, Vickers

115 HV
126 HV
225 HV
126 HV

Compressive Strength

230 MPa33.4 ksi
580 MPa84.1 ksi
260 MPa37.7 ksi

Hardness, Rockwell C

18 HRC

Same in both: Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,495°C2,723 °F
1,425°C2,597 °F
1,425°C2,597 °F
1,470°C2,678 °F

Liquidus Temperature

1,530°C2,786 °F
1,510°C2,750 °F
1,510°C2,750 °F
1,520°C2,768 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

52 W/m·K30 BTU/hr·ft·°F
51 W/m·K29.5 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F
51.9 W/m·K30 BTU/hr·ft·°F

Specific Heat Capacity

480 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
480 J/kg·K0.11 BTU/lb·°F
486 J/kg·K0.12 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12 µm/m·K6.7 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
12 µm/m·K6.7 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F

Latent Heat of Fusion

247 J/g106 BTU/lb
247 J/g106 BTU/lb
270 J/g116 BTU/lb
247 J/g106 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
350°C662 °F
400°C752 °F

Min Service Temperature

-20°C-4 °F
-20°C-4 °F
-40°C-40 °F
-20°C-4 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

10.5 % IACS
10.8 % IACS
9 % IACS
11 % IACS

Electrical Resistivity

1.65×10⁻⁷ Ω·m6.5 µΩ·in
1.6×10⁻⁷ Ω·m6.3 µΩ·in
1.9×10⁻⁷ Ω·m7.48 µΩ·in
1.6×10⁻⁷ Ω·m6.3 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.62 V
-0.65 V
-0.62 V
-0.65 V

Corrosion Resistance

10 / 100
10 / 100
12 / 100
10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

68 / 100
65 / 100
50 / 100
65 / 100

Machinability Rating (AISI 1212 = 100 %)

68%
70%
50%
72%

Weldability

95 / 100
95 / 100
75 / 100
95 / 100

Formability (cold)

80 / 100
78 / 100
65 / 100
80 / 100

Brazeability / Solderability

70 / 100
70 / 100
45 / 100
70 / 100

Polishability

40 / 100
45 / 100
45 / 100
40 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

26 MJ/kg11,178 BTU/lb
25 MJ/kg10,748 BTU/lb
25 MJ/kg10,748 BTU/lb
25 MJ/kg10,748 BTU/lb

Embodied Carbon (primary production)

2.1 kg CO₂/kg
1.9 kg CO₂/kg
2 kg CO₂/kg
2 kg CO₂/kg

Embodied Water

45 L/kg5.4 gal/lb
40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb

Typical Recycled Content

25%
30%
30%
40%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

39 kN·m/kg
54 kN·m/kg
84 kN·m/kg
57 kN·m/kg

Specific Stiffness (E / density)

26.1 MN·m/kg
25.5 MN·m/kg
25.5 MN·m/kg
25.5 MN·m/kg

Modulus of Resilience

140 kJ/m³
132 kJ/m³
841 kJ/m³
169 kJ/m³

Thermal Diffusivity

13.8 mm²/s
13.8 mm²/s
12.2 mm²/s
13.6 mm²/s

Thermal Shock Resistance Index

7
9
13
10

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleA283A656SPHCA36

Manufacturing and finishing

CapabilitySPHCA283A656A36
CNC machiningYesYesYes
Default conditionHRHRHRHR
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrNYesYesYes
AlTiNYesYesYes
CVD Al2O3YesYesYes
CVD TiCNYesYesYes
CVD TiNYesYesYes
CrNYesYesYes
DLCYesYesYes
HVOF CoatingYesYesYes
MoS2YesYesYes
Multilayer CVDYesYesYes
TiAlNYesYesYes
TiB2YesYesYes
TiCNYesYesYes
TiNYesYesYes
WC/CYesYesYes
ZrNYesYesYes

Both are offered for Sheet metal. They share 22 finishes: Black Oxide, Cerakote, Chrome Plating, Copper Plating, E-Coating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Hot-Dip Galvanizing, Manganese Phosphate, Nickel Plating and 10 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SPHC and A283 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.