FabDigit

SNCM220 vs SCM415 and 2 more: properties

SNCM220SCM41543204620

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

205 GPa29.7 Msi
206 GPa29.9 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Tensile Strength (Ultimate)

560 MPa81.2 ksi
640 MPa92.8 ksi
640 MPa92.8 ksi
570 MPa82.7 ksi

Yield Strength (0.2% offset)

385 MPa55.8 ksi
430 MPa62.4 ksi
415 MPa60.2 ksi
360 MPa52.2 ksi

Elongation at Break

29%
22%
22%
26%

Reduction in Area

60%
55%
50%
55%

Compressive Strength

385 MPa55.8 ksi
430 MPa62.4 ksi

Shear Strength

340 MPa49.3 ksi
400 MPa58 ksi
415 MPa60.2 ksi
380 MPa55.1 ksi

Fatigue Strength (Endurance Limit)

260 MPa37.7 ksi
290 MPa42.1 ksi
300 MPa43.5 ksi
260 MPa37.7 ksi

Fracture Toughness (K_IC)

95 MPa·√m86.5 ksi·√in
90 MPa·√m81.9 ksi·√in

Charpy V-Notch Impact (RT)

85 J62.7 ft·lbf
55 J40.6 ft·lbf
70 J51.6 ft·lbf
85 J62.7 ft·lbf

Hardness, Brinell

160 HB
180 HB
187 HB
163 HB

Hardness, Rockwell B

84 HRB
89 HRB
90 HRB
84 HRB

Hardness, Vickers

168 HV
190 HV

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,425°C2,597 °F
1,430°C2,606 °F
1,425°C2,597 °F
1,420°C2,588 °F

Liquidus Temperature

1,505°C2,741 °F
1,510°C2,750 °F
1,500°C2,732 °F
1,500°C2,732 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

46 W/m·K26.6 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F

Specific Heat Capacity

475 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

11.6 µm/m·K6.4 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Latent Heat of Fusion

260 J/g112 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
350°C662 °F
400°C752 °F

Min Service Temperature

-40°C-40 °F
-50°C-58 °F
-60°C-76 °F
-50°C-58 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

8.5 % IACS
7.8 % IACS
8 % IACS

Electrical Resistivity

2×10⁻⁷ Ω·m7.87 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.6 V
-0.61 V

Corrosion Resistance

12 / 100
12 / 100
11 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
58 / 100
50 / 100
57 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
60%
55%
65%

Weldability

55 / 100
55 / 100
40 / 100
65 / 100

Formability (cold)

60 / 100
60 / 100
45 / 100
58 / 100

Castability

40 / 100

Brazeability / Solderability

65 / 100
65 / 100
55 / 100
70 / 100

Polishability

60 / 100
60 / 100
60 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

30 MJ/kg12,898 BTU/lb
27 MJ/kg11,608 BTU/lb
31 MJ/kg13,328 BTU/lb
29 MJ/kg12,468 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
2.1 kg CO₂/kg
2.3 kg CO₂/kg
2.2 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
50 L/kg6 gal/lb
50 L/kg6 gal/lb
55 L/kg6.6 gal/lb

Same in both: Typical Recycled Content 30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

71 kN·m/kg
82 kN·m/kg
82 kN·m/kg
73 kN·m/kg

Specific Stiffness (E / density)

26.1 MN·m/kg
26.2 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

362 kJ/m³
449 kJ/m³
420 kJ/m³
316 kJ/m³

Thermal Diffusivity

12.3 mm²/s
11.9 mm²/s
11.8 mm²/s
12.3 mm²/s

Thermal Shock Resistance Index

11
11
12
11

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSCM41543204620SNCM220

Manufacturing and finishing

CapabilitySNCM220SCM41543204620
Default conditionHRHRHRHR
Relative cost$$ Standard$$ Standard$$$ Premium$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SNCM220 and SCM415 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.