FabDigit

Steel SCM422 vs SCM420 vs SCr445 vs SCM432

Benchmark · 4 materials

Side-by-side benchmark of 4 steel grades.

SCM422 vs SCM420 and 2 more: properties

SCM422SCM420SCr445SCM432

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

206 GPa29.9 Msi
207 GPa30 Msi
207 GPa30 Msi
207 GPa30 Msi

Tensile Strength (Ultimate)

580 MPa84.1 ksi
660 MPa95.7 ksi
1,030 MPa149 ksi
1,000 MPa145 ksi

Yield Strength (0.2% offset)

370 MPa53.7 ksi
440 MPa63.8 ksi
860 MPa125 ksi
850 MPa123 ksi

Elongation at Break

25%
22%
14%
17%

Reduction in Area

55%
52%
45%
56%

Shear Strength

360 MPa52.2 ksi
430 MPa62.4 ksi
620 MPa89.9 ksi
600 MPa87 ksi

Fatigue Strength (Endurance Limit)

280 MPa40.6 ksi
300 MPa43.5 ksi
480 MPa69.6 ksi
470 MPa68.2 ksi

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
40 J29.5 ft·lbf
45 J33.2 ft·lbf
60 J44.3 ft·lbf

Hardness, Brinell

170 HB
190 HB
302 HB
293 HB

Hardness, Rockwell B

87 HRB
91 HRB

Fracture Toughness (K_IC)

65 MPa·√m59.2 ksi·√in
60 MPa·√m54.6 ksi·√in
85 MPa·√m77.4 ksi·√in

Compressive Strength

880 MPa128 ksi
860 MPa125 ksi

Hardness, Rockwell C

32 HRC
31 HRC

Hardness, Vickers

318 HV
308 HV

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Density

7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.83 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,425°C2,597 °F
1,425°C2,597 °F
1,425°C2,597 °F
1,420°C2,588 °F

Liquidus Temperature

1,500°C2,732 °F
1,500°C2,732 °F
1,490°C2,714 °F
1,495°C2,723 °F

Thermal

How each material carries heat and how hot it can run.

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.2 µm/m·K6.8 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F

Max Service Temperature (continuous)

350°C662 °F
400°C752 °F
350°C662 °F
400°C752 °F

Min Service Temperature

-40°C-40 °F
-40°C-40 °F
-25°C-13 °F
-40°C-40 °F

Same in both: Thermal Conductivity 42 W/m·K24.3 BTU/hr·ft·°F · Latent Heat of Fusion 250 J/g107 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

8 % IACS
7.8 % IACS
8 % IACS
7.8 % IACS

Same in both: Electrical Resistivity 2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.62 V
-0.6 V
-0.62 V

Corrosion Resistance

10 / 100
12 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
60 / 100
42 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
62%
45%
55%

Weldability

40 / 100
55 / 100
25 / 100
45 / 100

Formability (cold)

55 / 100
60 / 100
20 / 100
40 / 100

Brazeability / Solderability

55 / 100
65 / 100
45 / 100
55 / 100

Polishability

60 / 100
60 / 100
60 / 100
65 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

34 MJ/kg14,617 BTU/lb
30 MJ/kg12,898 BTU/lb
30 MJ/kg12,898 BTU/lb
28 MJ/kg12,038 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.1 kg CO₂/kg
2.1 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

25%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

74 kN·m/kg
84 kN·m/kg
132 kN·m/kg
127 kN·m/kg

Specific Stiffness (E / density)

26.2 MN·m/kg
26.4 MN·m/kg
26.4 MN·m/kg
26.4 MN·m/kg

Modulus of Resilience

332 kJ/m³
468 kJ/m³
1,786 kJ/m³
1,745 kJ/m³

Thermal Diffusivity

11.4 mm²/s
11.4 mm²/s
11.3 mm²/s
11.3 mm²/s

Thermal Shock Resistance Index

10
11
17
16

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSCM420SCr445SCM422SCM432

Manufacturing and finishing

CapabilitySCM422SCM420SCr445SCM432
CNC machiningYes
Sheet metalYes
Default conditionHR
Relative cost$ Budget$$ Standard$ Budget$ Budget
Min. machined wall0.8 mm
Best machined surfaceRa 1.6 µm
AlCrNYes
AlTiNYes
Black OxideYes
CVD Al2O3Yes
CVD TiCNYes
CVD TiNYes
CerakoteYes
Chrome PlatingYes
CrNYes
DLCYes
E-CoatingYes
HVOF CoatingYes
Hot-Dip GalvanizingYes
MoS2Yes
Multilayer CVDYes
Nickel PlatingYes
PTFE CoatingYes
PaintingYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SCM422 and SCM420 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.