SCM415 vs 4320 and 2 more: properties

SCM41543204620SNCM220

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

206 GPa29.9 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Tensile Strength (Ultimate)

640 MPa92.8 ksi
640 MPa92.8 ksi
570 MPa82.7 ksi
560 MPa81.2 ksi

Yield Strength (0.2% offset)

430 MPa62.4 ksi
415 MPa60.2 ksi
360 MPa52.2 ksi
385 MPa55.8 ksi

Elongation at Break

22%
22%
26%
29%

Reduction in Area

55%
50%
55%
60%

Compressive Strength

430 MPa62.4 ksi
385 MPa55.8 ksi

Shear Strength

400 MPa58 ksi
415 MPa60.2 ksi
380 MPa55.1 ksi
340 MPa49.3 ksi

Fatigue Strength (Endurance Limit)

290 MPa42.1 ksi
300 MPa43.5 ksi
260 MPa37.7 ksi
260 MPa37.7 ksi

Fracture Toughness (K_IC)

90 MPa·√m81.9 ksi·√in
95 MPa·√m86.5 ksi·√in

Charpy V-Notch Impact (RT)

55 J40.6 ft·lbf
70 J51.6 ft·lbf
85 J62.7 ft·lbf
85 J62.7 ft·lbf

Hardness, Brinell

180 HB
187 HB
163 HB
160 HB

Hardness, Rockwell B

89 HRB
90 HRB
84 HRB
84 HRB

Hardness, Vickers

190 HV
168 HV

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,430°C2,606 °F
1,425°C2,597 °F
1,420°C2,588 °F
1,425°C2,597 °F

Liquidus Temperature

1,510°C2,750 °F
1,500°C2,732 °F
1,500°C2,732 °F
1,505°C2,741 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

44 W/m·K25.4 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F

Specific Heat Capacity

473 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F
11.6 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb
260 J/g112 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
350°C662 °F
400°C752 °F
400°C752 °F

Min Service Temperature

-50°C-58 °F
-60°C-76 °F
-50°C-58 °F
-40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.8 % IACS
8 % IACS
8.5 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2×10⁻⁷ Ω·m7.87 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.6 V
-0.61 V
-0.6 V

Corrosion Resistance

12 / 100
11 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

58 / 100
50 / 100
57 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
55%
65%
65%

Weldability

55 / 100
40 / 100
65 / 100
55 / 100

Formability (cold)

60 / 100
45 / 100
58 / 100
60 / 100

Brazeability / Solderability

65 / 100
55 / 100
70 / 100
65 / 100

Polishability

60 / 100
60 / 100
55 / 100
60 / 100

Castability

40 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

27 MJ/kg11,608 BTU/lb
31 MJ/kg13,328 BTU/lb
29 MJ/kg12,468 BTU/lb
30 MJ/kg12,898 BTU/lb

Embodied Carbon (primary production)

2.1 kg CO₂/kg
2.3 kg CO₂/kg
2.2 kg CO₂/kg
2.2 kg CO₂/kg

Embodied Water

50 L/kg6 gal/lb
50 L/kg6 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb

Same in both: Typical Recycled Content 30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

82 kN·m/kg
82 kN·m/kg
73 kN·m/kg
71 kN·m/kg

Specific Stiffness (E / density)

26.2 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

449 kJ/m³
420 kJ/m³
316 kJ/m³
362 kJ/m³

Thermal Diffusivity

11.9 mm²/s
11.8 mm²/s
12.3 mm²/s
12.3 mm²/s

Thermal Shock Resistance Index

11
12
11
11

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSCM41543204620SNCM220

Manufacturing and finishing

CapabilitySCM41543204620SNCM220
Default conditionHRHRHRHR
Relative cost$$ Standard$$$ Premium$$ Standard$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in SCM415 and 4320 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.